Environment-friendly paper-based material for radio frequency tag antenna and manufacturing method of environment-friendly paper-based material
A technology of radio frequency tags and manufacturing methods, applied in special paper, antenna support/installation device, paper, etc., can solve the problems that affect paper degradation, do not really solve the environmental pollution of electronic tags, and achieve the effect of easy evaporation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0073] Embodiment 1: a kind of manufacturing method of the described environment-friendly paper base material that is used for radio frequency tag antenna, comprises the steps:
[0074] Step 1, configuring a zein solution, and configuring the zein and a solvent to form a protein solution;
[0075] Specifically: when using ethanol with a volume concentration of 80-92%, the volume concentration of the protein in the protein solution is about 50-70%, but not limited thereto, such as, preferably, when using ethanol with a volume concentration of 92%, the protein The volume concentration of protein in the solution is about 65%;
[0076] The protein solution in step 1 may also include the following components: 10% by volume of citric acid, 3% by volume of polyglycerol fatty acid ester and 7% by volume of stearic acid;
[0077] Step 2, soaking the paper with the protein solution prepared in step 1;
[0078] The paper is coated paper;
[0079] Specifically: immerse the paper roll o...
Embodiment 2
[0083] Embodiment 2: a kind of manufacturing method of the described environment-friendly paper-based material that is used for radio frequency tag antenna, comprises the steps:
[0084] Step 1, configuring a prolamin solution, and configuring the prolamin and a solvent to form a protein solution;
[0085] Specifically: when using ethanol with a volume concentration of 80-92%, the volume concentration of the protein in the protein solution is about 50-70%, but not limited thereto, for example, preferably, when using ethanol with a volume concentration of 90%, The volume concentration of protein in the protein solution is about 65%;
[0086] The protein solution in step 1 may also include the following components: 3% by volume of citric acid, 7% by volume of polyglycerol fatty acid ester and 3% by volume of stearic acid;
[0087] Step 2, paper roller coating the protein solution prepared in step 1;
[0088] The paper is glassine paper;
[0089] Specifically: during the paper...
Embodiment 3
[0094] Embodiment 3: a kind of manufacturing method of the described environment-friendly paper-based material that is used for radio frequency tag antenna, comprises the steps:
[0095] Step 1, configure the coconut prolamin solution, and configure the coconut prolamin and solvent into a protein solution;
[0096] Specifically: when using ethanol with a volume concentration of 80-92%, the volume concentration of the protein in the protein solution is about 50-70%, but not limited thereto, for example, preferably, when using ethanol with a volume concentration of 90%, The volume concentration of protein in the protein solution is about 65%;
[0097] The protein solution in step 1 may also include the following components: 5% by volume of citric acid, 5% by volume of polyglycerol fatty acid ester and 5% by volume of stearic acid;
[0098] Step 2, spraying the paper with the protein solution prepared in step 1;
[0099] The paper is kraft paper;
[0100] Specifically: Spray t...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com