Artistic powder paint of mottle effect
A technology of powder coatings and markings, which is applied in the direction of art coatings, epoxy resin coatings, polyurea/polyurethane coatings, etc., can solve the problems of low mechanical properties of coatings, high comprehensive construction costs, environmental pollution, etc., and achieve production and use The effect of simple method
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] Raw material dosage (wt%)
[0023] Epoxy / polyester resin systems 60
[0024] Degasser 0.24
[0025] W-1 2
[0026] Carbon black 2.5
[0027] Ultrafine barium sulfate 18.4
[0028] Streaking agent 0.7
[0029] Pearlescent Pigment 4
[0030] Vapor SiO 2 0.1
[0031] Orientation aid 0.06
[0032] Artistic powder coating with mottled effect prepared according to the above formula. The coating adhesion is grade 0, the impact strength is 50cm, and the color difference between batches is ΔE≤1.
Embodiment 2
[0034] Raw material dosage (wt%)
[0035] Polyester / TGIC system 90
[0036] Degasser 0.4
[0037] W-1 2.8
[0038] Carbon black 2.8
[0039] Streaking agent 0.5
[0040] Pearlescent pigment 3.3
[0041] Vapor SiO 2 0.1
[0042] Orientation aid 0.1
[0043] Artistic powder coating with mottled effect prepared according to the above formula. Its coating adhesion is grade 0, impact strength 50cm, color difference between batches ΔE≤1, artificial accelerated aging time ≥500h, natural exposure for 12 months without blistering, rust, cracking, or peeling.
Embodiment 3
[0045] Raw material dosage (wt%)
[0046] Polyurethane Resin Systems 72
[0047] Degasser 0.2
[0048] W-1 2
[0049] Phthalo Green 6.7
[0050] Ultrafine Barium Sulfate 17
[0051] Streaking agent 1.5
[0052] Metallic Pigments 0.45
[0053] Al 2 o 3 C 0.1
[0054] Orientation aid 0.05
[0055] Artistic powder coating with mottled effect prepared according to the above formula. Its coating adhesion is grade 0, impact strength 50cm, color difference between batches ΔE≤1, artificial accelerated aging time ≥500h, natural exposure for 12 months without blistering, rust, cracking, or peeling.
PUM
Property | Measurement | Unit |
---|---|---|
Impact strength | aaaaa | aaaaa |
Impact strength | aaaaa | aaaaa |
Impact strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com