Biodegradable polypeptide vesicle loaded with hemoglobin and preparation method thereof
A technology of hemoglobin and biodegradation, applied in the direction of peptide/protein components, non-active components of polymer compounds, medical preparations containing active components, etc., can solve the problems of immunogenicity and rejection, and achieve excellent biological Effects of degradability, good stability and good compatibility
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0026] Embodiment 1: Synthesis of amino-terminated poly(N-benzyloxycarbonyl lysine) (PZLL)
[0027]Put 2.0g of N-benzyloxycarbonyllysine NCA into an ampoule baked by flame, ventilate with nitrogen three times, seal it and add 20ml of DMF with a syringe, after dissolving, add the DMF solution of n-hexylamine in proportion , Reacted in a 30°C oil bath for 72h with stirring. The reactant was settled with excess ether to obtain transparent and viscous PZLL, which was redissolved in chloroform and settled with excess ether to obtain a white solid. Pure amino-terminated PZLL was obtained by vacuum drying at 40°C for 24 hours.
Embodiment 2
[0028] Example 2: Synthesis of poly(Z-lysine)-polyphenylalanine two-block copolypeptide (PZLL-b-PPA)
[0029] Add the poly(Z-lysine) and phenylalanine NCA of the terminal amino group in proportion to the ampoule that has been baked with flame, and ventilate with nitrogen three times, add DMF (2wt%) with a syringe after sealing, and stir The reaction was carried out in an oil bath at 30° C. for 24 hours, and the subsequent treatment process was as shown in Example 1.
Embodiment 3
[0030] Example 3: Deprotection of PZLL-b-PPA
[0031] Deprotection of PZLL-b-PPA was achieved with hydrogen bromide. PZLL-b-PPA was dissolved in trifluoroacetic acid (0.04g / ml), then passed into hydrogen bromide gas, bubbling reaction for 30 minutes, continued stirring reaction in ice bath for 12 hours, and settled with excess ether to obtain the deprotected product. Vacuum-dried at 40°C for 24 hours to obtain polylysine-polyphenylalanine (PLL-b-PPA), its H NMR spectrum is shown in the attached Figure 4 .