Method for preparing fuel oil
A technology of fuel oil and coal tar, which is applied in the field of coal chemical industry, can solve the problems of low fuel oil efficiency, achieve the effects of small equipment investment, easy to master production technology, and high yield
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0029] Catalyst component: 50g of Y-type molecular sieve, 30ml of aqueous solution containing 0.8g of potassium bromide;
[0030] Preparation method: Immerse Y-type molecular sieve (produced by Wuxi Rongdeli Molecular Sieve Factory) with potassium bromide aqueous solution for 2 hours, and dry at 120°C for 2 hours to obtain a catalyst. The properties are shown in Table 1;
[0031] Potassium bromide in the catalyst is 1.21% of the weight of the catalyst in terms of bromine.
[0032] Utilize above-mentioned catalyzer to carry out the method for intermittent coal tar preparation fuel oil:
[0033] Add 300g of coal tar with a water content of 1wt% to the 1000ml autoclave device, and then add 4.5g of catalyst. After the autoclave is sealed, heat the autoclave to raise the temperature to 350°C, keep the temperature for 5 minutes, and then drop to room temperature Finally, the reaction product is taken out from the reactor, and then separated by distillation, and the fraction at 80-2...
Embodiment 2
[0037] Catalyst component: 50g of ZSM-5 molecular sieve, 25ml of aqueous solution containing 0.8g of potassium bromide;
[0038] Preparation method: ZSM-5 molecular sieve (produced by Zichuan Fenghuang Fine Chemical Co., Ltd., Zibo City) was impregnated with an aqueous solution of potassium bromide for 2 hours, and dried at a temperature of 120°C for 2 hours to obtain a catalyst. The properties are shown in Table 1;
[0039] Potassium bromide in the catalyst is 1.21% of the weight of the catalyst in terms of bromine.
[0040] Utilize above-mentioned catalyzer to carry out the method for intermittent coal tar preparation fuel oil:
[0041] Add 300g of coal tar with a moisture content of 0.1wt% to the 1000ml autoclave device, and then add 4.5g of catalyst. After the reactor is sealed, heat the reactor to raise the temperature to 360°C, keep the temperature for 10 minutes, and then drop to room temperature Finally, the reaction product is taken out from the reactor, and then sep...
Embodiment 3
[0045] Catalyst component: γ-Al 2 o 3 50g 30ml of aqueous solution containing 1.0g of potassium bromide;
[0046] Preparation method: γ-Al 2 o 3 Immerse it in an aqueous solution of potassium bromide for 2 hours, and dry it for 1 hour at a temperature of 120°C to obtain a catalyst whose properties are shown in Table 1;
[0047] Potassium bromide in the catalyst is 1.66% of the weight of the catalyst in terms of bromine.
[0048] Utilize above-mentioned catalyzer to carry out the method for intermittent coal tar preparation fuel oil:
[0049] Add 300g of coal tar with a water content of 1.8wt% to the 1000ml autoclave device, and then add 4.5g of catalyst. After the reactor is sealed, heat the reactor to raise the temperature to 350°C, keep the temperature for 15 minutes, and then drop to room temperature Finally, the reaction product is taken out from the reactor, and then separated by distillation, and the fraction at 80-280° C. is taken to obtain fuel oil;
[0050] Uti...
PUM
Property | Measurement | Unit |
---|---|---|
density | aaaaa | aaaaa |
dew point | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com