Non-wood fiber raw material cooking auxiliary agent and preparation process thereof
A technology of non-wood fibers and cooking aids, which is applied in cellulose raw material pulping, fiber raw material processing, textile and paper making, etc., can solve problems such as inapplicability, and achieve the effect of reducing dosage, obvious effect and improving strength
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0040] A preparation process for cooking aids for non-wood fiber raw materials, comprising the following steps:
[0041] Step 1, weighing 1 part of anthraquinone, 2 parts of sodium dodecylbenzenesulfonate, 5 parts of fatty alcohol polyoxyethylene ether, 10 parts of dimethylsulfonic acid, and 2 parts of hydroxylamine according to the weight ratio;
[0042] Step 2: Prepare all the ingredients in Step 1 in proportion and add them to the reaction kettle, start stirring, and raise the temperature to 60°C and keep it warm for 150 minutes;
[0043] Step 3, then add 2 parts of sodium carbonate to the reaction kettle in step 2 for neutralization, react for 70 minutes, and keep stirring, and finally cool to 30°C to discharge the finished product.
Embodiment 2
[0045] A preparation process for cooking aids for non-wood fiber raw materials, comprising the following steps:
[0046] Step 1, weighing 3 parts of anthraquinone, 3 parts of sodium dodecylbenzenesulfonate, 6 parts of fatty alcohol polyoxyethylene ether, 15 parts of dimethylsulfonic acid, and 5 parts of hydroxylamine according to the weight ratio;
[0047] In step 2, prepare all the ingredients in step 1 in proportion and add them to the reaction kettle, start stirring, and raise the temperature to 80°C, and keep it warm for 100 minutes;
[0048] Step 3, then add 5 parts of sodium carbonate to the reaction kettle in step 2 for neutralization, react for 60 minutes, and keep stirring, and finally cool to 35°C to discharge the finished product.
Embodiment 3
[0050] A preparation process for cooking aids for non-wood fiber raw materials, comprising the following steps:
[0051] Step 1, weighing 5 parts of anthraquinone, 4 parts of sodium dodecylbenzenesulfonate, 10 parts of fatty alcohol polyoxyethylene ether, 30 parts of dimethylsulfonic acid, and 8 parts of hydroxylamine according to the weight ratio;
[0052] Step 2, prepare all the ingredients in step 1 and add them to the reaction kettle in proportion, start stirring, and raise the temperature to 100°C and keep it warm for 60 minutes;
[0053] Step 3, then add 10 parts of sodium carbonate to the reaction kettle in step 2 for neutralization, react for 90 minutes, and keep stirring, and finally cool to 40°C to discharge the finished product.
[0054] The non-wood fiber raw material cooking aid of the present invention overcomes the disadvantage of traditional anthraquinone being insoluble in cooking liquid in terms of performance, has good solubility and permeability, can improv...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com