Lacquer wax sizing agent and preparation method thereof
A technology of sizing agent and lacquer wax, which is applied in the direction of wax addition and water repellent addition, can solve the problems of poor antibacterial property, poor barrier and water resistance, low toxicity, etc., to improve smoothness and strength indicators, Good barrier and water resistance effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0029] The composition and weight percentage of the lacquer wax sizing agent are: 5% lacquer wax, 5% starch, 1% reinforcing agent (0.5% hydroxyethyl cellulose, 0.5% hemicellulose), 0.2% chitosan, 0.01% acetic acid %, the remainder is water.
[0030] The preparation method of the present embodiment paint wax sizing agent is as follows:
[0031] (1) Add 250g of water to 50g of lacquer wax, stir at 85°C and 100r / min for 30min to emulsify, and emulsify for later use;
[0032] (2) Add 250g of water to 50g of starch, stir at 85°C and 100r / min for 30min to boil the gelatin, and set aside after boiling the gelatin;
[0033] (3) Add 60g of water to 10g of enhancer (5g of hydroxyethyl cellulose, 5g of hemicellulose) to dissolve, set aside;
[0034] (4) After preparing 0.1g of acetic acid with water to make a solution with a mass percentage concentration of 1%, it is used to dissolve 2g of chitosan, mix the chitosan solution with the solution of step (3) and stir evenly, then add it to...
Embodiment 2
[0039] The composition and mass percentage of this lacquer wax sizing agent are: lacquer wax 1%, modified starch 3%, reinforcing agent (0.2% carboxymethyl cellulose, acetylated hemicellulose 0.4%) 0.6%, chitosan 0.4%, hydrochloric acid 0.02%, and the rest is water.
[0040] (1) Add 40g of water to 10g of lacquer wax, stir at 95°C and 30r / min for 200min to emulsify, and emulsify for later use;
[0041] (2) Add 240g of water to 30g of modified starch, stir at 65°C and 80r / min for 60min to boil the glue, and set aside after boiling the glue;
[0042] (3) Add 60g of water to 6g of enhancer (2g of carboxymethyl cellulose, 4g of acetylated hemicellulose) to dissolve and set aside;
[0043] (4) After preparing 0.2g of hydrochloric acid with water into a solution with a concentration of 3% by mass, it is used to dissolve 4g of chitosan, and the chitosan solution and the solution of step (3) are mixed and stirred evenly, then added to the mixing tank, and finally Add the solutions in...
Embodiment 3
[0048] The composition and mass percentage of the lacquer wax sizing agent are: 3% lacquer wax, 0.5% modified starch, 0.8% hemicellulose as a reinforcing agent, 0.5% chitosan, 0.015% citric acid, and the rest is water.
[0049] (1) Add 135g of water to 30g of lacquer wax, stir at 55°C and 300r / min for 100min to emulsify, and emulsify for later use;
[0050] (2) Add 50g of water to 5g of modified starch, stir at 55°C and 40r / min for 80min to boil the gelatin, and set aside after boiling the gelatin;
[0051] (3) Add 40g of water to 8g of enhancer hemicellulose to dissolve, set aside;
[0052] (4) After preparing 0.15g of citric acid with water into a solution with a mass percent concentration of 5%, it is used to dissolve 5g of chitosan, and the chitosan solution and the solution of step (3) are mixed and stirred evenly, and then added to the mixing tank. Finally, add the solutions in step (1) and step (2) into the mixing tank, make up the total amount of water, and stir evenl...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com