A semi-dull high-strength low-elongation viscose fiber and its preparation method
A viscose fiber, high-strength and low-elongation technology, which is applied in the field of semi-dull high-strength and low-elongation viscose fiber and its preparation, can solve the problem that the market share of viscose fiber has decreased, and there is no greater demand for downstream new textile development and industrial upgrading. And other problems, to achieve high product strength, good color fastness of finished products, and good uniformity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0063] The pulp raw material is sequentially soaked, ground, crushed, kneaded, depolymerized, yellowed, dissolved, filtered, defoamed, matured, matting agent is added, spinning and drawing, refining and drying to obtain semi-dull viscose. Adhesive fiber, the semi-dull high-strength low-elongation viscose adhesive fiber of the present embodiment has the following performance index system:
[0064] The dry breaking strength is 3.12 cN / dtex, the wet breaking strength is 1.65cN / dtex,
[0065] The strength required to produce 5% elongation in wet state is 0.55cN / dtex,
[0066] Dry elongation at break is 19.0%, wet elongation at break is 21.0%,
[0067] The crystallinity is 40%, the radial water swelling degree is 22%, and the content of matting agent is 0.15%.
[0068] The linear density deviation rate is -11.0%, the residual sulfur is 8.0mg / 100g,
[0069] The length deviation rate is -11.0%, the ultra-long fiber rate is 0.48%, and the whiteness is 84.1%.
[0070] The double-le...
Embodiment 2
[0072] The difference between the semi-dull high-strength low-elongation viscose fiber of the present embodiment and embodiment 1 is: the present embodiment has the following indicators:
[0073] The dry breaking strength is 3.15 cN / dtex, the wet breaking strength is 1.67cN / dtex,
[0074] The strength required to produce 5% elongation in wet state is 0.54cN / dtex,
[0075] The dry elongation at break is 18.9%, and the wet elongation at break is 20.8%.
[0076] The crystallinity is 40%, the radial water swelling degree is 22.5%, and the content of matting agent is 0.3%.
[0077] The whiteness is 84.6%, the linear density deviation rate is -10.0%, the residual sulfur is 8.0mg / 100g,
[0078] The length deviation rate is +10.0%, and the ultra-long fiber rate is 0.5%,
[0079] The double-length fiber is 4.0mg / 100g, and the defect is 4.0mg / 100g.
Embodiment 3
[0081] In order to better implement the present invention, this embodiment further provides a specific preparation method of a semi-dull high-strength low-elongation viscose fiber of the present invention, and measures performance indicators.
[0082] A method for preparing semi-dull high-strength and low-elongation viscose fiber: the pulp raw material is soaked and pressed to remove the lye to obtain alkali cellulose; the prepared alkali cellulose is crushed, kneaded, and depolymerized to remove the lye Obtain methyl cellulose; the obtained methyl cellulose is yellowed to obtain cellulose sulfonate; the obtained cellulose sulfonate is dissolved in a solvent, filtered, matured, defoamed, and a spinning solution is obtained; Add the matting agent to the obtained spinning solution and send it to the spinning machine for spinning and drafting to obtain tow, and the tow is refined and dried to obtain the viscose fiber of the present invention. Samples were taken, and each index wa...
PUM
Property | Measurement | Unit |
---|---|---|
pulverization | aaaaa | aaaaa |
strength | aaaaa | aaaaa |
pulverization | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com