Red low-angle-dependence zinc sulfide structure color materials and preparation method thereof
A zinc sulfide, low-angle technology, applied in the direction of zinc sulfide, etc., can solve the problems of reducing structural color dependence, difficult to widely use, film quality influence, etc., to achieve no angle dependence, process operation process is simple and easy to solve, Easy to fade effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0027] The present invention is achieved through the following technical solutions:
[0028] A preparation method of a low-angle-dependent red zinc sulfide structural color pigment, comprising the following steps:
[0029] 1) Weigh Zn(NO 3 ) 2 ·6H 2 O and polyvinylpyrrolidone (PVP) several grams, add in the beaker, according to the ratio 0.03gPVP:100mL deionized water, total water volume is 100mL magnetic stirring fully dissolves and evenly mixes, and stirs 30min to obtain uniform solution;
[0030] 2) Accurately weigh 0.3 g of thioacetamide, add 50 mL of deionized water and ultrasonically mix for 10-20 minutes to obtain an aqueous solution of thioacetamide;
[0031] 3) Stir the above two homogeneous solutions of 1) and 2) respectively, add them into the same beaker, and react in a water bath at 80°C for 6 hours under magnetic stirring to obtain an emulsion containing zinc sulfide microspheres, and then wash with water , alcohol washing three times and ultrasonic dispersio...
Embodiment 2
[0035] 1) Weigh Zn(NO 3 ) 2 ·6H 2 O and polyvinylpyrrolidone (PVP) several grams, add in the beaker, according to the ratio 0.02gPVP:100mL deionized water, total water volume is 100mL magnetic stirring fully dissolves and evenly mixes, and stirs 30min to obtain uniform solution;
[0036] 2) Accurately weigh 0.3 g of thioacetamide, add 50 mL of deionized water and ultrasonically mix for 10-20 minutes to obtain an aqueous solution of thioacetamide;
[0037]3) Stir the above two homogeneous solutions of 1) and 2) respectively, add them into the same beaker, and react in a water bath at 70° C. for 8 hours under magnetic stirring to obtain an emulsion containing zinc sulfide microspheres. After washing with water and washing with alcohol for three times, ultrasonic dispersion is carried out to obtain an ethanol solution of monodisperse zinc sulfide microspheres;
[0038] 4) Dry the ethanol solution of monodisperse zinc sulfide microspheres prepared in step 3) in a vacuum oven at...
Embodiment 3
[0040] 1) Weigh Zn(NO 3 ) 2 ·6H 2 O and polyvinylpyrrolidone (PVP) several grams, add in the beaker, according to the ratio 0.03gPVP:100mL deionized water, total water volume is 100mL magnetic stirring fully dissolves and evenly mixes, and stirs 30min to obtain uniform solution;
[0041] 2) Accurately weigh 0.4 g of thioacetamide, add 50 mL of deionized water and ultrasonically mix for 10-20 minutes to obtain an aqueous solution of thioacetamide;
[0042] 3) Stir the above two homogeneous solutions of 1) and 2) respectively, add them into the same beaker, and react in a water bath at 85° C. for 5 hours under magnetic stirring to obtain an emulsion containing zinc sulfide microspheres. After washing with water and washing with alcohol for three times, ultrasonic dispersion is carried out to obtain an ethanol solution of monodisperse zinc sulfide microspheres;
[0043] 4) Dry the ethanol solution of monodisperse zinc sulfide microspheres prepared in step 3) in a vacuum oven a...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com