A technology for mine transportation and rails, which is applied in the field of mine car rails for mine transportation. It can solve problems such as low hardness of mine car rails, short service life, safety accidents, etc., and achieve simple and feasible preparation process, improved mechanical properties, and good corrosion resistance. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0018] A mine car track for mine transportation, which is prepared from the following raw materials in parts by weight:
[0019] 1 part of vanadium oxide (Vanadium(IV) oxide, also known as vanadium pentoxide) powder, 2 parts of magnesium powder, 3 parts of glass fiber, 5 parts of titanium carbide powder, 10 parts of nickel powder, 12 parts of copper powder, 15 parts of niobium powder, 15 parts of graphite powder, 30 parts of tungsten powder, 30 parts of aluminum powder, 1000 parts of iron powder. The particle diameters of the above raw materials are all controlled within 100um.
[0020] The preparation method of above-mentioned track comprises the steps:
[0021] 1) Weigh each raw material according to the weight part for later use;
[0022] 2) Add glass fiber and graphite powder to acetone in turn, stir at 100 rpm for 6 hours, and then refrigerate at 4°C for 12 hours to obtain auxiliary materials; among them, the mass of acetone is twice that of graphite powder;
[0023] 3...
Embodiment 2
[0026] A mine car track for mine transportation, which is prepared from the following raw materials in parts by weight:
[0027] 2 parts of vanadium oxide (Vanadium(IV) oxide, alias alum pentoxide) powder, 3 parts of magnesium powder, 5 parts of glass fiber, 8 parts of titanium carbide powder, 15 parts of nickel powder, 18 parts of copper powder, 20 parts of niobium powder, 20 parts of graphite powder, 40 parts of tungsten powder, 40 parts of aluminum powder, and 1200 parts of iron powder. The particle diameters of the above raw materials are all controlled within 100um.
[0028] The preparation method of above-mentioned track comprises the steps:
[0029] 1) Weigh each raw material according to the weight part for later use;
[0030] 2) Add glass fiber and graphite to acetone in turn, stir at 100 rpm for 6 hours, and then refrigerate at 4°C for 12 hours to obtain auxiliary materials; among them, the mass of acetone is twice that of graphite powder;
[0031] 3) Mix vanadium...
Embodiment 3
[0034] 1. Mechanical performance test: GCr15 alloy steel commonly used in the market is used as the control group, and three groups are respectively set up: 1 is the embodiment 1 group, 2 is the embodiment 2 group, and 3 is the control group; the specific test results are shown in Table 1:
[0035] Table 1
[0036]
[0037] Conclusion: The track prepared by the invention shows good performance in terms of tensile strength, hardness, bending strength, elongation after break, hardness and impact energy, etc., which fully meets the needs of mine transportation.
[0038] 2. According to GB10124-1988 metal material laboratory uniform corrosion full immersion test method, put the sample prepared in the above embodiment obliquely in the 3.5% NaCl solution, take it out after 4 days with CrO3+AgNO3+Ba(NO3)2+distilled water Remove the corrosion products on the surface of the sample, then clean it with acetone and absolute alcohol, and measure the corrosion rate (mm / a).
[0039] The ...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com