[0019] A preparation method of a pressure-bearing plugging agent for drilling fluid comprises the following steps:
[0020] (1) First extract the cracked fiber of rice straw: separate the leaves, stems and ears of the rice straw raw material, discard the leaves and ears, cut the stem into 3-5cm, soak in 5% sodium bicarbonate solution for 24 hours, take out , keep the moisture content 10-15%, and then expand the rod through the expansion equipment to obtain the straw cracked fiber in the form of cotton ball;
[0021] (2) Preparation of modified asphalt:
[0022] First mix 360kg of water with 22kg of dodecyl dimethyl benzyl ammonium chloride, then thoroughly mix them through an emulsifier to form a soap solution and heat it to 65°C; then grind and mix the soap solution with 580kg of 90# asphalt through a colloid mill To obtain emulsified asphalt, then quickly mix the emulsified asphalt with 38kg of liquid fluorosilicone rubber heated to 40°C in a mixer, and stir thoroughly to o...
Embodiment 2
[0026] The preparation of rice straw pyrolysis fiber and modified asphalt is as in Example 1.
[0027] Preparation of pressure-bearing plugging agent for drilling fluid
[0028] According to the proportion by weight, take 40 parts of walnut shell powder, 30 parts of rice straw cracked fiber, 4 parts of calcium carbonate powder, 1 part of hydrolyzed polyacrylonitrile ammonium salt, 4 parts of instant sodium silicate, 6 parts of aluminum stearate, carboxylate 5 parts of methyl cellulose, 5 parts of redispersible latex powder, 10 parts of modified asphalt, mixed in a mixing device for 1 hour, dried at a constant temperature of 60°C, and granulated. The average particle size is 20-300 mesh. The pressure-bearing plugging agent for drilling fluid is obtained.
[0029] Example 2
[0030] The preparation of rice straw pyrolysis fiber and modified asphalt is as in Example 1.
[0031] Preparation of pressure-bearing plugging agent for drilling fluid
[0032] According to the ratio b...