A mixing tank and concrete technology, which is applied in the field of fluorine coatings, can solve the problems of corrosion of the inner wall of the mixing tank and shorten the service life of the mixing tank, and achieve the effects of preventing concrete corrosion, prolonging the service life, and having excellent corrosion resistance and wear resistance.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] (1) Add 5 parts of furfural slag to 2 times the weight of water, add sodium bicarbonate to adjust the pH value of the solution to 7-8 after soaking for 8 hours, then use a filter press to press filter, wash the obtained filter residue three times, and then send it to a freeze dryer. Pulverize into powder after fully drying to obtain material I;
[0025] (2) Add 25 parts of ultra-fine polytetrafluoroethylene powder and 8 parts of polyamide resin to 30 parts of butyl acetate, mix well and let stand for 30 minutes, then heat to reflux state and keep stirring for 15 minutes, then add 5 parts of polyamide resin while hot Butylene terephthalate and 3 parts of C5 petroleum resin are mixed uniformly to obtain material II;
[0026] (3) Add 10 parts of fluorocarbon resin and 6 parts of water-white rosin pentaerythritol ester to 30 parts of cyclohexanone, and heat to reflux state and insulate and stir for 15 minutes, then add 3 parts of toughening agent, 5 parts of hydrogenated ro...
Embodiment 2
[0032] (1) Add 9 parts of furfural slag to 2 times the weight of water, add sodium bicarbonate to adjust the pH value of the solution to 7-8 after soaking for 8 hours, then use a filter press to filter, wash the obtained filter residue three times, and then send it to a freeze dryer. Pulverize into powder after fully drying to obtain material I;
[0033] (2) Add 25 parts of ultra-fine polytetrafluoroethylene powder and 8 parts of polyamide resin to 35 parts of butyl acetate, mix well and let stand for 30 minutes, then heat to reflux state and keep stirring for 15 minutes, then add 4 parts of polyamide resin while hot Butylene terephthalate and 5 parts of C5 petroleum resin are mixed uniformly to obtain material II;
[0034] (3) Add 15 parts of fluorocarbon resins and 5 parts of water-white rosin pentaerythritol esters to 30 parts of cyclohexanone, and heat to reflux state and insulate and stir for 15 minutes, then add 5 parts of tougheners, 4 parts of hydrogenated rosin glycer...
PUM

Abstract
Description
Claims
Application Information

- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com