Thermal insulation mortar and manufacturing method thereof
A technology of thermal insulation mortar and sand, applied in the field of building materials, can solve the problems of compression resistance, low flexural strength, low tensile strength, poor toughness, etc., and achieve the effect of enhancing continuity, improving toughness, and reducing cracks
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] A thermal insulation mortar is composed of the following raw materials in parts by weight:
[0023] 25 parts of cement, 30 parts of sand, 10 parts of lime powder, 8 parts of lightweight aggregate, 5 parts of expansion agent, 4 parts of anti-crack additive, 2 parts of water reducing agent, 8 parts of polyvinyl alcohol, hydroxypropyl methylcellulose 6 parts of vegetable matter, 6 parts of zeolite powder, and 15 parts of straw fiber.
[0024] A method for producing thermal insulation mortar, comprising the following steps:
[0025] Step 1: Accurately weigh various raw materials according to the weight ratio, first mix cement, sand, lime powder, lightweight aggregate, expansion agent, anti-cracking additive, straw fiber and zeolite powder in the mixer;
[0026] Step 2: Pour an appropriate amount of water into the mixer, and add water reducer, polyvinyl alcohol and hydroxypropyl methylcellulose, and continue to stir evenly to make a mortar.
Embodiment 2
[0028] A thermal insulation mortar is composed of the following raw materials in parts by weight:
[0029] 25 parts of cement, 32 parts of sand, 15 parts of lime powder, 10 parts of lightweight aggregate, 8 parts of expansion agent, 7 parts of anti-cracking additive, 5 parts of water reducing agent, 9 parts of polyvinyl alcohol, hydroxypropyl methylcellulose 7 parts of vegetable matter, 11 parts of zeolite powder, and 17 parts of straw fiber.
[0030] A method for producing thermal insulation mortar, comprising the following steps:
[0031] Step 1: Accurately weigh various raw materials according to the weight ratio, first mix cement, sand, lime powder, lightweight aggregate, expansion agent, anti-cracking additive, straw fiber and zeolite powder in the mixer;
[0032] Step 2: Pour an appropriate amount of water into the mixer, and add water reducer, polyvinyl alcohol and hydroxypropyl methylcellulose, and continue to stir evenly to make a mortar.
Embodiment 3
[0034] A thermal insulation mortar is composed of the following raw materials in parts by weight:
[0035] 30 parts of cement, 40 parts of sand, 18 parts of lime powder, 12 parts of lightweight aggregate, 9 parts of expansion agent, 8 parts of anti-crack additive, 6 parts of water reducing agent, 10 parts of polyvinyl alcohol, hydroxypropyl methylcellulose 8 parts of vegetable, 7 parts of zeolite powder, 16 parts of straw fiber.
[0036] A method for producing thermal insulation mortar, comprising the following steps:
[0037] Step 1: Accurately weigh various raw materials according to the weight ratio, first mix cement, sand, lime powder, lightweight aggregate, expansion agent, anti-cracking additive, straw fiber and zeolite powder in the mixer;
[0038] Step 2: Pour an appropriate amount of water into the mixer, and add water reducer, polyvinyl alcohol and hydroxypropyl methylcellulose, and continue to stir evenly to make a mortar.
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com