Problems solved by technology

But there is no mention of increasing the plasticizing effect of chlorinated par

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Modified chlorinated paraffin, preparation method and application thereof
  • Modified chlorinated paraffin, preparation method and application thereof
  • Modified chlorinated paraffin, preparation method and application thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0023] A preparation method of modified chlorinated paraffin, comprising the steps of:

[0024] S1. Dissolve 1 part of chlorinated paraffin in 10 parts of acetone by weight. After the chlorinated paraffin is completely dissolved, add 1 part of thiosalicylic acid and 2 parts of potassium carbonate, and react at a temperature of 90°C under nitrogen protection. After 24 hours, after the reaction is completed, pour the reactant into 10 parts of ethanol / water (the volume ratio of ethanol and water is 2:1) mixed solution, and dry in vacuum for 2 hours to obtain a transparent liquid;

[0025] S2. Dissolving the above transparent liquid in 10 parts of tetrahydrofuran, adjusting the pH value to 4 with hydrochloric acid, then pouring into 10 parts of ethanol for extraction, and drying in vacuum for 2 hours to obtain a transparent liquid thiosalicylic acid modified chlorinated paraffin product;

[0026] S3. Add 1 part of thiosalicylic acid-modified chlorinated paraffin product to 10 part...

Embodiment 2

[0028] A preparation method of modified chlorinated paraffin, comprising the steps of:

[0029] S1. Take 2 parts by weight of chlorinated paraffin and dissolve in 15 parts of acetone. After the chlorinated paraffin is completely dissolved, add 2 parts of thiosalicylic acid and 2 parts of potassium carbonate, and react at a temperature of 70°C under nitrogen protection. After 24 hours, after the reaction is completed, the reactant is poured into 15 parts by weight of ethanol / water (the volume ratio of ethanol and water is 2:1) mixed solution, and vacuum-dried for 2 hours to obtain a transparent liquid;

[0030] S2. Dissolving the above transparent liquid in 15 parts of tetrahydrofuran, adjusting the pH value to 4 with hydrochloric acid, pouring into 10 parts of ethanol for extraction, and drying in vacuum for 2 hours to obtain a transparent liquid thiosalicylic acid-modified chlorinated paraffin product;

[0031] S3. Add 2 parts of thiosalicylic acid-modified chlorinated paraff...

Embodiment 3

[0033] A preparation method of modified chlorinated paraffin, comprising the steps of:

[0034] S1. Take 2 parts by weight of chlorinated paraffin and dissolve in 20 parts of acetone. After the chlorinated paraffin is completely dissolved, add 2 parts of thiosalicylic acid and 2 parts of potassium carbonate, and react at a temperature of 70°C under nitrogen protection. 24h, after the reaction is completed, the reactant is poured into 20 parts of ethanol / water (the volume ratio of ethanol and water is 2:1) mixed solution, and vacuum-dried for 2h to obtain a transparent liquid;

[0035] S2. Dissolving the above transparent liquid in 20 parts of tetrahydrofuran, adjusting the pH value to 4 with hydrochloric acid, pouring into 20 parts of ethanol for extraction, and drying in vacuum for 2 hours to obtain a transparent liquid thiosalicylic acid-modified chlorinated paraffin product;

[0036] S3. Add 2 parts of thiosalicylic acid-modified chlorinated paraffin product to 10 parts of ...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention discloses a preparation method of modified chlorinated paraffin, which comprises the following steps: dissolving chlorinated paraffin in a solvent, adding thiosalicylic acid and potassium carbonate, reacting at 50-100 DEG C under the protection of nitrogen, pouring that reactants into an ethanol solution, and performing vacuum drying to obtain a transparent liquid; dissolving the clear liquid in a solvent and adjusting the pH to 4-5, pouring into ethanol to extract, vacuum drying to obtain thiosalicylic acid modified chlorinated paraffin product; adding the chlorinated paraffin modified by thiosalicylic acid into solvent, then adding epoxy fatty acid methyl ester and N,N-dimethyl formamide, performing reflux reaction at 50-80 DEG C, pouring into ethanol to extract, vacuum drying to obtain modified chlorinated paraffin. The invention also discloses a modified chlorinated paraffin. The invention also discloses the application of a modified chlorinated paraffin in a plasticizer. The modified chlorinated paraffin prepared by the invention is environmentally friendly, has good compatibility with organic substances and good plasticizing effect, and can improve the deficiency of the traditional chlorinated paraffin.

Description

technical field [0001] The invention relates to the technical field of modified chlorinated paraffin, in particular to a modified chlorinated paraffin and its preparation method and application. Background technique [0002] Chlorinated paraffin is a traditional auxiliary plasticizer for polyvinyl chloride, but its plasticizing effect is poor, and it is easy to remove HCl under the action of light or heat during use, resulting in a decrease in its own polarity, resulting in a reaction with polyvinyl chloride. The resin compatibility gradually decreases, and the products gradually harden. Therefore, the application of chlorinated paraffin in the field of plasticizers is limited. The preparation of modified chlorinated paraffin plasticizers with good plasticizing effects will broaden its application fields and increase product additions. value is significant. [0003] CN 201810719663.7 discloses a bisphenol-A modified heat-resistant chlorinated paraffin and its preparation me...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
IPC IPC(8): C10G73/38
CPCC10G73/38
Inventor 王中立王西弱王文本王西宇
Owner ANHUI XINGXIN CHEM TECH
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products