UV-radiation-curable precious-metal preparation, transfer pictures containing said preparation, and process for decoration
A radiation-curing, precious-metal technology for applications in metal-free paints, decorative arts, and processes for producing decorative surface effects, capable of solving problems such as non-exhibiting color indirect printing reactivity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0055] Example 1: Hybrid system
[0056] Thiol gold (about 40% gold) 21%
[0057] Sulfurized Alkylphenolic Resin 16%
[0058] Trimethylolpropane Monoformal Acrylate 30%
[0059] 3,4-Epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate 20.5%
[0060] Rhodium naphthenate (5% rhodium) 2.5%
[0061] [4-(2-Methylpropyl)phenyl](4-methylphenyl)iodonium-hexafluorophosphate 4.5%
[0062] Bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide 2.5%
[0063] 2-Hydroxy-2-methyl-1-phenylacetone 2.5%
[0064] Defoamer Byk 088 0.5%
Embodiment 2
[0065] Embodiment 2: cationic system
[0066] Thiol gold (about 40% gold) 32%
[0067] Sulfurized Alkylphenolic Resin 5%
[0068] Rhodium naphthenate (5% rhodium) 1%
[0069] Chromium naphthenate (5% Cr 2 o 3 ) 0.3%
[0070] Bismuth naphthenate (5% Bi 2 o 3 ) 1.6%
[0071] 3,4-Epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate 51%
[0072] Triarylsulfonium hexafluorophosphate 7%
[0073] [4-(2-Methylpropyl)phenyl](4-methylphenyl)iodonium-hexafluorophosphate 1%
[0074] Defoamer Byk 088 1.1%
[0075] All components are dissolved in the monomer with stirring at a temperature of up to 80°C.
Embodiment 3
[0076] Example 3: Polished Gold Preparation
[0077] The bright gold of embodiment 2 85.54
[0078] Gold Dust 14.26
[0079] Lead borosilicate 0.20
[0080] The feed was homogenized in a ball mill for 48 hours.
[0081] The formulations described above (Examples 1-2) were printed on a Trucal brand transfer paper on a Fleischle printer using a screen (e.g. polyester 120-31 (thread count-yarn diameter [μm]) or 165-31), Curing in a UV dryer was followed by filming thereon with a commercial film solution (product number: 80 450, Ferro GmbH) and polyester screen 27-120. Adsorb the transfer decal paper pattern onto the porcelain, and then fire it at 820°C by conventional firing method, with a heating rate of 400K / h, a retention time of 10 minutes, and a cooling rate of 400K / h; or rapid firing at 880°C For firing, the heating rate is 1600K / h, the retention time is 1 minute, and the cooling rate is 1600K / h. Obtain decorative objects with a fine sheen.
[0082] The formulation of...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com