An environmentally friendly, water-based technology, applied in paper coatings, polyester coatings, polyurea/polyurethane coatings, etc., can solve the problems of restricting the application range of colored coatings, environmental pollution in production and use, and high content of volatile organic compounds. The effect of low cost, good printing adaptability, and good solvent resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0048] A preparation method of an environment-friendly water-based coloring paint, the method comprising the following steps:
[0049] (1) Prepare materials according to the following components and content (parts by weight):
[0050] components
parts by weight
Water-based resin acrylic modified polyurethane emulsion
40
Co-solvent ethanol
10
Deionized water
46.25
Coalescent n-butanol
3
pH adjuster ammonia water
0.2
Anti-abrasion agent silica sol
0.1
Wetting agent nonylphenol polyoxyethylene ether
0.2
Rheology control agent hydrophobically modified alkali-swellable acrylic acid
0.2
Defoamer Modified Polysiloxane
0.05
[0051] (2) Put the water-based resin into the reaction kettle, and stir evenly at a low speed of 300-500 rpm;
[0052] (3) After mixing the co-solvent, deionized water and film-forming aids evenly, add them to the reaction kettle w...
Embodiment 2
[0058] A preparation method of an environment-friendly water-based coloring paint, the method comprising the following steps:
[0059] (1) Prepare materials according to the following components and content (parts by weight):
[0060] components
parts by weight
Water-based resin acrylic emulsion
60
Co-solvent isopropanol
15
[0061] Deionized water
21.5
Coalescent propylene carbonate
1
pH adjuster 2-Amino-2-methyl-1-propanol
(AMP-95)
0.2
Anti-abrasion agent polyethylene emulsified wax
2
Wetting agent acetylene glycol
0.1
Defoamer modified silicone defoamer
0.2
[0062] The Tg of the acrylic emulsion is 50°C and the molecular weight is 500,000;
[0063] (2) Put the water-based resin into the reaction kettle, and stir evenly at a low speed of 300-500 rpm;
[0064] (3) After mixing the co-solvent, deionized water, and film-forming aids evenly, add them to...
Embodiment 3
[0070] A preparation method of an environment-friendly water-based coloring paint, the method comprising the following steps:
[0071] (1) Prepare materials according to the following components and content (parts by weight):
[0072] components
parts by weight
Water-based resin water-based polyester
50
Co-solvent propylene glycol monomethyl ether
25
Deionized water
23.1
pH adjuster ammonia water
0.2
Anti-abrasion agent polyether silicone
1
Wetting agent nonylphenol polyoxyethylene ether
0.5
[0073] Rheology Control Agent Condensed Polyurethane Emulsion
0.1
0.1
[0074] The Tg of water-based polyester is 30°C and the molecular weight is 50,000;
[0075] (2) Put the water-based resin into the reaction kettle, and stir evenly at a low speed of 300-500 rpm;
[0076] (3) After mixing the co-solvent, deionized water and film-forming a...
PUM
Property | Measurement | Unit |
---|---|---|
Tg | aaaaa | aaaaa |
Softening point | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com