Method for preparing thermoplastic vulcanized rubber

A thermoplastic vulcanizate and equipment technology, applied in the field of thermoplastic vulcanizate preparation, can solve the problems of decreased elastic properties, reduced hardness and fluidity, and difficulty in uniform dispersion and extrusion of materials, so as to reduce equipment investment and production costs, improve Dispersion and performance, the effect of improving blending efficiency

Inactive Publication Date: 2010-11-24
GUANGZHOU SCUT BESTRY TECHNOLOGY CO LTD
View PDF6 Cites 7 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0004] To a certain extent, dynamic vulcanization technology is not very suitable for preparing thermoplastic vulcanizates with low hardness and high fluidity, because low hardness TPV is generally obtained by increasing the rubber content. With the increase of rubber content, the plastic matrix must form a continuous Phase becomes difficult and the prepared material becomes difficult to uniformly disperse and extrude
High-fluidity TPV is generally obtained by increasing the plastic content or using high-melting plastic materials. Increasing the plastic content will increase the fluidity of TPV, but the hardness and compression deformation of TPV will also increase, and the elastic properties will decrease. At the same time, the viscosity during melt blending will also decrease, and the use of plastics with high melting index will also reduce the viscosity during melt blending. When the viscosity is too low, it is not conducive to the shear dispersion of rubber, and even the rubber cannot be used. fully vulcanized
In addition, increasing the amount of softener can also reduce hardness and increase fluidity, but when the amount of softener is large, it will also affect the dispersion of TPV and the vulcanization of rubber
Therefore, the above problems are some difficulties in the preparation of TPV, no matter whether it is blended with an ordinary internal mixer or an ordinary twin-screw extruder to produce TPV. Although, these problems can be solved by using more advanced processing equipment, such as Germany The latest TPV production equipment produced by Berstorff, the countercurrent pump in the mixing can make the rubber and other components more uniformly dispersed, and the bypass feeding equipment and metering system are also introduced on the twin-screw extruder to facilitate vulcanization. The late addition of agent and late oil filling and other processes, but this requires the purchase of expensive TPV special production equipment

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Method for preparing thermoplastic vulcanized rubber
  • Method for preparing thermoplastic vulcanized rubber
  • Method for preparing thermoplastic vulcanized rubber

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0026] Utilize common rubber and plastic equipment including common internal mixer and heating temperature control system thereof, open mill, plastic crusher and plastic extruder, prepare the EPDM rubber / polypropylene (EPDM / polypropylene) of rubber-plastic ratio 80 / 20 PP) thermoplastic vulcanizate. The heating and temperature control system of the ordinary internal mixer in the ordinary rubber equipment is high-temperature heat transfer oil heating or steam heating, and the heating control temperature range is 100-220°C. In this embodiment, the model is ML-5L meshing type with intelligent control system The internal mixer heating and temperature control system is changed from hot water circulation heating to high-temperature heat conduction oil heating, so that the maximum heating control temperature of the internal mixer can reach 220°C, so as to meet the blending of plastics with higher melting points.

[0027] The improved plastic vulcanizate internal mixer blending process...

Embodiment 2

[0039] Utilize common rubber and plastic equipment including common internal mixer and heating and temperature control system thereof, open mill, plastic crusher and plastic extruder, prepare the EPDM rubber / polypropylene (EPDM / polypropylene) of rubber-plastic ratio 60 / 40 PP) thermoplastic vulcanizate, the equipment that present embodiment uses is with embodiment one.

[0040] The improved plastic vulcanizate internal mixer blending process includes the following steps and process conditions:

[0041] Step 1: Pre-preparation of rubber compound

[0042] Prepare materials by mass: oil-extended EPDM rubber 150 (including 50 parts of naphthenic oil), white carbon black 45, antioxidant RD 2, stearic acid 1.5, softener naphthenic oil 50, organic peroxide DCP 3 , cross-linking additive TAIC 3, polypropylene plastic 67;

[0043] Mix EPDM rubber, white carbon black, anti-aging agent, stearic acid, 30 parts of naphthenic oil, cross-linking aids and organic peroxides on the open mill a...

Embodiment 3

[0052] Using ordinary rubber and plastic equipment including ordinary internal mixer and its heating and temperature control system, open mill, plastic crusher and plastic extruder, etc., prepare high fluidity, rubber-plastic ratio 55 / 45 styrene-butadiene rubber / high-density polymer Polyethylene (SBR / HDPE) thermoplastic vulcanizate, the equipment used in this embodiment is the same as that of embodiment one.

[0053] The improved plastic vulcanizate internal mixer blending process includes the following steps and process conditions:

[0054] Step 1: Pre-preparation of rubber compound

[0055] Prepare materials by mass: oil-extended styrene-butadiene rubber 137.5 (containing 37.5 parts of oil), zinc oxide 3, stearic acid 2, antioxidant RD 2, white carbon black 45, carbon black N3308, softener naphthenic oil 50, sulfur 1.7 , Accelerator TT 1.8, HDPE 82;

[0056] Mix oil-extended styrene-butadiene rubber, zinc oxide, stearic acid, anti-aging agent, white carbon black, N330, 30 ...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

PropertyMeasurementUnit
melting pointaaaaaaaaaa
Login to view more

Abstract

The invention discloses a method for preparing thermoplastic vulcanized rubber and provides technology for preparing the thermoplastic vulcanized rubber by only using common rubber and plastic equipment. The common rubber and plastic equipment comprises a common rubber kneading machine and a heating temperature control system thereof, an open mill, a plastic crusher and a plastic extruder, wherein the temperature range of the heating temperature control system of the common rubber kneading machine is controlled to be between 100 and 220 DEG C; the blending process of the thermoplastic vulcanized rubber kneading machine comprises the following steps of: firstly pre-preparing rubber mixing glue; then blending the rubber mixing glue with the rubber kneading machine; and adding the mixture bysteps when the using amount of a softening agent or plastic is over 25 percent of the total capacity of mixing. The method creates a precedent of preparing the thermoplastic vulcanized rubber by using the common rubber and plastic equipment. The properties such as tensile strength, tear strength, dispersion, extrusion appearance and the like of the prepared thermoplastic vulcanized rubber are obvious better than those of the thermoplastic vulcanized rubber prepared by the prior art. Meanwhile, the method reduces equipment investment and production cost for TPV manufacturers.

Description

technical field [0001] The invention relates to the preparation technology of thermoplastic vulcanizate, in particular to a method for preparing thermoplastic vulcanizate by utilizing ordinary rubber and plastic equipment. Background technique [0002] As we all know, thermoplastic vulcanizate is a blended thermoplastic elastomer prepared by dynamic full vulcanization technology. When rubber and thermoplastic resin are melted and mixed, the rubber is completely chemically cross-linked "in situ" by means of a vulcanizing agent. Under the action of force, the cross-linked rubber is broken into a large number of micro-particles, which are dispersed in the continuous thermoplastic resin matrix to form a "sea-island" structure, thus becoming a thermoplastic vulcanizate, namely TPV (Theromoplastic Vulcanizate). The rubber used to prepare TPV usually includes: natural rubber, trans isoprene rubber, styrene-butadiene rubber, butadiene rubber, EPDM rubber, nitrile rubber, butyl rubbe...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): B29B7/28C08L23/16C08L23/12C08L9/06C08L23/06C08J3/24
CPCB29B7/183B29B7/28B29B7/7495B29B7/823
Inventor 禤文权张海邹明清李彦均
Owner GUANGZHOU SCUT BESTRY TECHNOLOGY CO LTD
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products