An environmentally friendly, glue-spraying technology, used in adhesives, shellac adhesives, other rubber adhesives, etc., can solve problems such as rebound phenomenon, furniture rework and glue, affect work efficiency, etc., to improve work efficiency and save drying time. , spraying effect uniform effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0009] (1) First put quantitative 5# petroleum distillate, butane, propane, and dimethyl ether into the agitator, and stir until fully uniform to become a mixed solution;
[0010] (2) Quantitative synthetic resin is dropped into the stirrer again and continues to stir;
[0011] (3) Put quantitative natural resin, synthetic rubber, concentrated all-purpose glue, synthetic solution, butyl fat and a small amount of preservative into the agitator and continue to stir and dissolve for 5 hours;
[0012] (4) Check that all materials are completely dissolved into light yellow glue, and then filter through 80 mesh.
Embodiment 2
[0014] (1) First put quantitative 5# petroleum distillate, butane, propane, and dimethyl ether into the agitator, and stir until fully uniform to become a mixed solution;
[0015] (2) Quantitative synthetic resin is dropped into the stirrer again and continues to stir;
[0016] (3) Put quantitative natural resin, synthetic rubber, concentrated all-purpose glue, synthetic solution, butyl fat and a small amount of preservative into the agitator and continue to stir and dissolve for 5.5 hours;
[0017] (4) Check that all materials are completely dissolved into light yellow glue, and then filter through 80 mesh.
Embodiment 3
[0019] (1) First put quantitative 5# petroleum distillate, butane, propane, and dimethyl ether into the agitator, and stir until fully uniform to become a mixed solution;
[0020] (2) Quantitative synthetic resin is dropped into the stirrer again and continues to stir;
[0021] (3) Put quantitative natural resin, synthetic rubber, concentrated all-purpose glue, synthetic solution, butyl fat and a small amount of preservative into the agitator and continue to stir and dissolve for 6 hours;
[0022] (4) Check that all materials are completely dissolved into light yellow glue, and then filter through 80 mesh.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com