Iron mine oxidized ore flotation green collector and production process thereof

A collector and ore-oxidizing technology, applied in flotation, solid separation and other directions, can solve the problems of low iron-bearing tailings re-selection rate, unstable beneficiation index, low average raw ore grade, etc. Outstanding impurity removal effect and outstanding iron extraction effect

Inactive Publication Date: 2014-05-21
肖国光 +1
View PDF5 Cites 15 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

China's iron ore resources are relatively poor, especially compared with Brazil and Australia, the main iron ore exporting countries, my country's iron ore resources have the following obvious deficiencies: ①The average raw ore grade is low; ②The proportion of rich ore is relatively small; ③SiO 2 ④ Iron ore contains phosphorus, sulfur and arsenic exceeding t

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Iron mine oxidized ore flotation green collector and production process thereof
  • Iron mine oxidized ore flotation green collector and production process thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0034] A kind of iron ore flotation anion collector of the present invention, this collector is formulated by the component of following quality: 32g of hydroxy peroxide monoethanolamine, hogwash oil monoethanolamine 8g, 8-hydroxyquinoline 10g, cyclodextrin 10g, cetyl alcohol 15g, emulsifier OP-10 2g and water 23g.

[0035] The specific preparation method of the collector in this embodiment is: first synthesize the main agent of hydroxy peroxy oleic acid monoethanolamine and hogwash oil monoethanolamine through organic reaction, and then combine 35 g of hydroxy peroxy oleic acid monoethanolamine and hogwash oil monoethanolamine with the above-mentioned mass The rest of the components (namely adjuvant) are mixed and stirred evenly to obtain the microemulsion type collector of the present invention (number RA-925).

[0036] The application method of the collector in this embodiment is: first dilute the above-mentioned collector with water into a collector solution with a mass co...

Embodiment 2

[0043] An anion collector for iron ore flotation of the present invention, the collector is mainly prepared from the following components: C3 ~ C22 linear and / or branched mixed hydroxy fatty acid diethanolamine 47g, 4-methyl -8-hydroxyquinoline 5g, B-cyclodextrin 5g, oxidized kerosene 13g, diesel oil 5g, emulsifier SP-80 3g and water 22g. (No. RA-935)

[0044] The specific preparation method of the collector in this example is: first synthesize 47g of C3~C22 straight chain and / or branched chain mixed hydroxyl fatty acid diethanolamine main agent through organic reaction, and then C3~C22 straight chain and / or branched mixed hydroxyl 47g of fatty acid diethanolamine is mixed with the rest of the above-mentioned quality components (ie adjuvant) and stirred evenly to obtain the microemulsion type collector of the present invention. The preparation process produces no waste gas, waste water and waste residue.

[0045] The application method of the collector in this embodiment i...

Embodiment 3

[0051] A kind of iron ore flotation anion collector of the present invention, this collector is mainly formulated by the following components of quality: 53g of hydroxysoyate triethanolamine, 3g of 6-methyl-8-hydroxyquinoline, γ - Cyclodextrin 2g, myristyl alcohol 10g, diesel oil 7g, emulsifier Triton 100 5g and water 20g (code RA-945).

[0052] The specific preparation method of the collector in this example is as follows: first synthesize the main agent of oxidized hydroxysoyate triethanolamine through organic reaction, and then mix 53 g of the main agent hydroxysoyate triethanolamine with the remaining components (i.e. auxiliary agents) of the above quality, And stir evenly, make the collector of microemulsion type of the present invention.

[0053] The application method of the collector in this example is as follows: first dilute the above-mentioned collector with water into a collector solution with a mass concentration of 2%, and then use the collector solution as taili...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention relates to an iron mine and oxidized ore beneficiation and flotation agent and a production method thereof and specifically discloses an iron ore and oxidized mine flotation anion collector; the main preparing agents of the anion collector are fatty acid modifier and derivatives thereof; assisting agents of the collector also comprise fatty alcohol, emulsifier and water. The production method of the collector comprises the following steps of compounding the main agents by organic action, then weighting rest components according to certain mass fractions, mixing according to a certain sequence, and uniformly stirring to prepare the micro-emulsion homogeneous phase viscous liquid. The collector has the advantages of strong collecting capacity, strong argillization resistance, low production cost, hard water resistance, stable performances, small agent use level, good selectivity, environment friendliness, safety and adaptivity to low temperature. By changing the variety and use level of the main agents, the series of collectors can be used for the flotation of diversified iron mines, phosphorite mines, fluorites, tungsten mines, rare earth mines, ilmenites and diversified oxidized mines.

Description

technical field [0001] The invention belongs to the technical field of high-efficiency utilization of mineral resources, and in particular relates to a flotation reagent for beneficiation of iron ore and various oxidized ores, a preparation method and application thereof. Background technique [0002] Mineral resources are one-time resources and are non-renewable. Due to years of mining and utilization, all kinds of rich ore resources in the world are decreasing day by day. Refractory minerals will become more and more important. Most ore resources in my country generally have the characteristics of "poor, fine, miscellaneous" and high impurity content, while high-quality "ore concentrate" has broad application prospects and broad market prospects, which objectively requires the concentrator to choose a reasonable capture Collector and its flotation process to produce high-quality concentrate, so as to achieve maximum economic benefits and save resources. Not only that, hig...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
IPC IPC(8): B03D1/004B03D101/02
Inventor 肖国光周智勇陶林芝王新水
Owner 肖国光
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products