Preparation method for high-performance steel shots
A high-performance, steel shot technology, applied in the field of metal abrasives, can solve the problems of reduced utilization, low added value, waste of resources, etc., to improve impact resistance and wear resistance, increase strength and ductility, reduce The effect of processing costs
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] Example 1 Preparation of high-performance steel shot with a diameter of 0.15 mm
[0021] (1) Sorting scrap steel wire ropes (No. 72 steel, S≤0.04wt%, P≤0.04wt%) according to the diameter of the single wire to obtain scrap steel wire ropes with the same single wire diameter;
[0022] (2) Use a wire dismantling machine to disassemble the waste steel wire ropes of the same diameter obtained through sorting into steel wires. When dismantling, the length of each steel wire is disassembled to 100m;
[0023] (3) Send the disassembled steel wire into a hydrogen annealing furnace for annealing at 400°C for 5 minutes;
[0024] (4) Straighten the annealed steel wire, and then perform cold drawing to a diameter of 0.1515mm (a positive tolerance of 10‰ than the target steel shot diameter);
[0025] (5) Cut the cold-drawn steel wire into a cylinder with a length of 0.1515mm;
[0026] (6) The surface of the cylinder obtained by cutting in step (5) is subjected to polishing and grind...
Embodiment 2
[0027] Example 2 Preparation of high-performance steel shot with a diameter of 2.4 mm
[0028] (1) Sorting scrap steel wire ropes (No. 45 steel, S≤0.04wt%, P≤0.04wt%) according to the diameter of the single wire to obtain scrap steel wire ropes with the same single wire diameter;
[0029] (2) Use a wire dismantling machine to dismantle the waste steel wire ropes of the same diameter obtained through sorting into steel wires. When dismantling, the length of each steel wire is disassembled to 1000m;
[0030] (3) Send the disassembled steel wire into a hydrogen annealing furnace for annealing at 700°C for 2 minutes;
[0031] (4) Straighten the annealed steel wire, and then perform cold drawing to a diameter of 2.412mm (a positive tolerance of 5‰ more than the target steel shot diameter);
[0032] (5) Cut the cold-drawn steel wire into a cylinder with a length of 2.412mm;
[0033] (6) The surface of the cylinder obtained by cutting in step (5) is subjected to polishing and grind...
Embodiment 3
[0034] Example 3 Preparation of high-performance steel shot with a diameter of 1.5mm
[0035] (1) Sorting scrap steel wire ropes (No. 60 steel, S≤0.04wt%, P≤0.04wt%) according to the diameter of the single wire to obtain scrap steel wire ropes with the same single wire diameter;
[0036] (2) Use a wire dismantling machine to dismantle the waste steel wire ropes of the same diameter obtained through sorting into steel wires. When dismantling, the length of each steel wire is disassembled to 500m;
[0037] (3) Send the disassembled steel wire into a hydrogen annealing furnace for annealing at 600°C for 3 minutes;
[0038] (4) Straighten the annealed steel wire, and then perform cold drawing to a diameter of 1.512mm (a positive tolerance of 8‰ more than the target steel shot diameter);
[0039] (5) Cut the cold-drawn steel wire into a cylinder with a length of 1.512mm;
[0040] (6) The surface of the cylinder obtained by cutting in step (5) is subjected to polishing and grindin...
PUM
Property | Measurement | Unit |
---|---|---|
diameter | aaaaa | aaaaa |
diameter | aaaaa | aaaaa |
diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com