Pink crystal bead embryo and preparation method thereof
A crystal bead, pink technology, applied in the field of pink crystal bead and its preparation, can solve the problems of poor coloring, environmental pollution, uneven color, etc., and achieve reduced production costs, good production efficiency, and bright colors Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0017] A kind of pink crystal bead embryo of the present invention, this pink crystal bead embryo is made up of the following proportioning components by weight: 95 parts of quartz sand, 9 parts of zinc oxide, 26 parts of soda ash, 18 parts of potassium carbonate, 8 parts of boric acid, 2.5 parts of calcium carbonate, 1 part of aluminum hydroxide, 1 part of table salt, 15 parts of potassium nitrate, 0.008 parts of gold chloride, 0.001 part of silver nitrate, 1.5 parts of antimony trioxide and 1 part of cerium oxide.
[0018] The preparation process of the pink crystal bead embryo is as follows:
[0019] 1) Extract 95 parts by weight of quartz sand, 9 parts of zinc oxide, 26 parts of soda ash, 18 parts of potassium carbonate, 8 parts of boric acid, 2.5 parts of calcium carbonate, 1 part of aluminum hydroxide, 1 part of table salt, and 15 parts of potassium nitrate , 0.008 parts of gold chloride, 0.001 parts of silver nitrate, 1.5 parts of antimony trioxide and 1 part of cerium ...
Embodiment 2
[0025] It is different from embodiment 1 in that this pink crystal bead embryo is made up of the following proportions by weight: 165 parts of quartz sand, 17 parts of zinc oxide, 48 parts of soda ash, 30 parts of potassium carbonate, 15 parts of boric acid, carbonic acid 5.5 parts of calcium, 3 parts of aluminum hydroxide, 2 parts of table salt, 27 parts of potassium nitrate, 0.015 parts of gold chloride, 0.003 parts of silver nitrate, 3.5 parts of antimony trioxide and 5 parts of cerium oxide.
Embodiment 3
[0027] It is different from embodiment 1 in that this pink crystal bead embryo is made up of the following proportioning components in parts by weight: 155 parts of quartz sand, 11 parts of zinc oxide, 38 parts of soda ash, 30 parts of potassium carbonate, 12 parts of boric acid, carbonic acid 3 parts of calcium, 1.5 parts of aluminum hydroxide, 1 part of table salt, 21 parts of potassium nitrate, 0.009 parts of gold chloride, 0.001 parts of silver nitrate, 2.3 parts of antimony trioxide and 1.8 parts of cerium oxide.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com