Preparation method for gravure ink connecting emulsion for water-based OPP packaging film
A packaging film and gravure technology, applied in the chemical industry, can solve problems such as human injury and environmental pollution, and achieve the effects of strong printing adaptability, good anti-adhesion, and fast drying
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] Add 100 grams of water into a four-neck flask, raise the temperature to 75°C, weigh 5 grams of K12 and dissolve it in 20 grams of hot water, mix MMA, BA, DAAM and MAA in a ratio of 1:1:0.1:0.1 and weigh 20g Add it into the K12 solution to stir and emulsify, then slowly add the above-mentioned emulsion into the four-necked flask, and at the same time dissolve the initiator APS in an appropriate amount of water, add the initiator to the above solution, and the mass percentage of the initiator APS is the above-mentioned 1~2% of the solution mass; gradually add it dropwise into a four-neck flask, and finish the drop within 40-50 minutes. The reaction is carried out under normal pressure for 1 hour. After the reaction, the liquid becomes transparent and has blue opalescence, then heats up to 85°C ;
[0017] BA, MMA, MAA, DAAM and DDM are mixed and emulsified according to a mass ratio of 1:1:0.1:0.1:0.05, and then 80g is added dropwise to the above-mentioned four-necked flask...
Embodiment 2
[0021] The invention provides a kind of preparation method of water-based OPP packaging film gravure ink connection emulsion, comprising the following steps:
[0022] 1) Add 100 parts by weight of water into a reaction vessel and raise the temperature to 70~80°C as base water;
[0023] 2) Dissolve 5 parts by weight of sodium dodecylsulfonate into 20 parts by weight of hot water at 60-85°C, and mix methyl methacrylate, butyl acrylate, diacetone acrylamide and methacrylic acid according to 1 : 1:0.1:0.1 mass ratio after mixing, weigh 20 parts by weight and add to sodium dodecylsulfurate solution, stir and emulsify; then set aside.
[0024] 3) Slowly add the emulsion in step 2) into the four-necked flask, and at the same time dissolve the initiator ammonium persulfate in water. The mass percent concentration of the ammonium persulfate solution is 10-40%. agent, the mass percentage of the initiator is 1-2% of the above-mentioned solution mass; slowly add it into the above-mention...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com