Wool setting agent and preparation method thereof
A sizing agent and wool technology, which is applied in the field of textiles, can solve the problems of wool fabrics being easy to wrinkle, affect wool fabrics, and easy deformation, etc., and achieve low volatility, excellent washing fastness, and smooth surface
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0044] The invention discloses a wool setting agent, which comprises the following components according to important parts: 1 part of ammonium thioglycolate, 3 parts of polyethylene glycol octylphenyl ether, 2 parts of tartaric acid, and 1 part of aluminum stearate , 3 parts of acetylated lanolin, 1 part of hydroxymethyl cellulose, 5 parts of sodium citrate, 10 parts of sodium secondary alkylsulfonate, 5 parts of magnesium chloride, 1 part of urea, and 20 parts of deionized water.
[0045] The present invention also provides a kind of preparation method of wool setting agent, and concrete steps comprise:
[0046] Step 1, add 20 parts of deionized water into the reaction kettle, heat in an oil bath, under nitrogen environment, condense and reflux, and raise the temperature to 70°C;
[0047] Step 2, add 1 part of ammonium thioglycolate and 3 parts of polyethylene glycol octylphenyl ether, stir at 500 rpm for 5 minutes;
[0048] Step 3, adding an appropriate amount of pH regulat...
Embodiment 2
[0056] The invention discloses a wool setting agent, which comprises the following components according to the important parts: 2 parts of ammonium thioglycolate, 4 parts of polyethylene glycol octylphenyl ether, 3 parts of tartaric acid, and 2 parts of aluminum stearate , 4 parts of acetylated lanolin, 2 parts of hydroxymethyl cellulose, 6 parts of sodium citrate, 13 parts of sodium secondary alkyl sulfonate, 6 parts of magnesium chloride, 2 parts of urea, 25 parts of deionized water.
[0057] The present invention also provides a kind of preparation method of wool setting agent, and concrete steps comprise:
[0058] Step 1, add 25 parts of deionized water into the reaction kettle, heat in an oil bath, under nitrogen environment, condense and reflux, and raise the temperature to 75°C;
[0059] Step 2, add 2 parts of ammonium thioglycolate and 4 parts of polyethylene glycol octylphenyl ether, stir at 800 rpm for 8 minutes;
[0060] Step 3, adding an appropriate amount of pH r...
Embodiment 3
[0068] The invention discloses a wool setting agent, which comprises the following components according to important parts: 3 parts of ammonium thioglycolate, 5 parts of polyethylene glycol octylphenyl ether, 4 parts of tartaric acid, and 3 parts of aluminum stearate , 5 parts of acetylated lanolin, 3 parts of hydroxymethyl cellulose, 7 parts of sodium citrate, 15 parts of sodium secondary alkylsulfonate, 7 parts of magnesium chloride, 3 parts of urea, and 30 parts of deionized water.
[0069] The present invention also provides a kind of preparation method of wool setting agent, and concrete steps comprise:
[0070] Step 1, add 30 parts of deionized water into the reaction kettle, heat in an oil bath, under nitrogen environment, condense and reflux, and raise the temperature to 80°C;
[0071] Step 2, add 3 parts of ammonium thioglycolate and 5 parts of polyethylene glycol octylphenyl ether, stir at 1000 rpm for 10 minutes;
[0072] Step 3, adding an appropriate amount of pH ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com