A processing method and technology of bamboo products, which are applied in the field of bamboo products, can solve the problems of poor adhesion strength of surface coating film, easy swelling of bamboo fibers, poor waterproof effect, etc., and achieve high adhesion strength, difficult peeling, and enhanced insect repellent effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0023] A processing method for waterproof bamboo products, comprising the steps of:
[0024] S1, slice the bamboo, remove green and yellow, and dry to obtain bamboo slices;
[0025] S2. Mix 1 part of quaternary ammonium copper and 200 parts of water evenly in parts by weight, then add 30 parts of bamboo chips, stand at high temperature for 4 hours, the temperature of standing at high temperature is 90 ° C, and separate solid and liquid to obtain pretreated bamboo;
[0026] S3, drying the pretreated bamboo, placing it in a carbonization furnace for carbonization treatment for 30 minutes, the pressure of carbonization treatment is 0.2Mpa, filtering, immersing in the mixed oil, taking it out, drying, and then coating the surface with pretreatment varnish, curing, drying, Woven to obtain waterproof bamboo products.
[0027] The mixed oil comprises by weight: 40 parts of castor oil, 2 parts of grapeseed oil, 4 parts of ethylene glycol, and 2 parts of polyethylene wax.
[0028] Th...
Embodiment 2
[0031] A processing method for waterproof bamboo products, comprising the steps of:
[0032] S1, slice the bamboo, remove green and yellow, and dry to obtain bamboo slices;
[0033] S2. Mix 3 parts of quaternary ammonium copper and 100 parts of water evenly in parts by weight, then add 50 parts of bamboo chips, stand at high temperature for 2 hours, the temperature of standing at high temperature is 98 ° C, and separate solid-liquid to obtain pretreated bamboo;
[0034] S3, drying the pretreated bamboo, placing it in a carbonization furnace for carbonization for 20 minutes, the pressure of the carbonization treatment is 0.5Mpa, filtering, immersing in the mixed oil, taking it out, drying, and then coating the surface with a pretreatment varnish, curing, drying, Woven to obtain waterproof bamboo products.
[0035] The mixed oil comprises by weight: 20 parts of castor oil, 10 parts of grapeseed oil, 1 part of ethylene glycol, and 4 parts of polyethylene wax.
[0036] The pretr...
Embodiment 3
[0039] A processing method for waterproof bamboo products, comprising the steps of:
[0040] S1, slice the bamboo, remove green and yellow, and dry to obtain bamboo slices;
[0041] S2. Mix 1.5 kg of quaternary ammonium copper and 180 kg of water evenly, then add 35 kg of bamboo slices, stand at high temperature for 3.5 hours, the temperature of standing at high temperature is 92°C, and separate solid and liquid to obtain pretreated bamboo;
[0042] S3, drying the pretreated bamboo, placing it in a carbonization furnace for carbonization for 28 minutes, the pressure of the carbonization treatment is 0.3Mpa, filtering, immersing in the mixed oil, taking it out, drying, and then coating the surface with a pretreatment varnish, curing, drying, Woven to obtain waterproof bamboo products.
[0043] The mixed oil includes: castor oil 35kg, grape seed oil 4kg, ethylene glycol 3kg, polyethylene wax 2.5kg.
[0044]The pretreatment varnish is prepared by the following process: add 1kg ...
PUM
Property | Measurement | Unit |
---|---|---|
Thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com