High proportion red mud building material
A technology of building materials and high mixing ratio, applied in the field of building materials, can solve the problems of low utilization rate of red mud, high energy consumption, low red mud content, etc., and achieve the effect of excellent flexural strength
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0062] Embodiment 1: the modifying agent is a phosphoric acid modifying agent; it is 30 parts of phosphoric acid modifying agent and 60-360 parts of fly ash by mass fraction. Preferably, by mass fraction, it is 30 parts of phosphoric acid modifier and 180 parts of fly ash. Preferably, the phosphoric acid modifier is a phosphoric acid solution with a concentration of 25% by mass.
[0063] For embodiment 1, be divided into five groups and carry out performance test, five groups of specific proportioning situations are shown in the following table:
[0064]
[0065] Perform performance tests for the above five groups, the test results are shown in the table below or see Figure 1-3 Shown:
[0066]
Embodiment 2
[0067] Embodiment 2 also includes silicon powder; it is 20-100 parts of silicon powder by mass fraction.
[0068] For embodiment 2, be divided into five groups and carry out performance test, five groups of specific proportioning situations are shown in the following table:
[0069]
[0070] The performance test was carried out for the above five groups, and the test results are shown in the table below:
[0071]
Embodiment 3
[0072] Embodiment 3, described modifying agent is phosphoric acid modifying agent, sodium citrate modifying agent and oxalic acid modifying agent; In terms of mass fraction, 4.98 parts of phosphoric acid modifying agent, 15 parts of sodium citrate modifying agent, 25.12 parts oxalic acid modifier and 30-150 parts of fly ash. Preferably, by mass fraction, it is 4.98 parts of phosphoric acid modifier, 15 parts of sodium citrate modifier, 25.12 parts of oxalic acid modifier and 60 parts of fly ash.
[0073] Wherein, the phosphoric acid modifier is a phosphoric acid solution with a concentration of 25% by mass. The sodium citrate modifier is a sodium citrate solution with a mass percent concentration of 20-25%. The oxalic acid modifier is an oxalic acid solution with a concentration of 20-25% by mass.
[0074] For embodiment 3, be divided into five groups and carry out performance test, five groups of specific proportioning situations are shown in the following table:
[0075] ...