A water-based paint and preparation technology, applied in the direction of epoxy resin paint, coating, etc., can solve the problems of inability to improve night vision, high raw material prices, and no self-leveling ability, so as to achieve improved night vision, low price, The effect of low manufacturing cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0027] refer to figure 1 , a preparation process of water-based paint, specifically comprising the following steps:
[0028] S1. Select raw materials: select the following components by weight: 300 parts of water, 100 parts of acrylic resin, 150 parts of epoxy resin, 10 parts of fluorescent powder, 20 parts of ethylene glycol, 20 parts of propylene glycol methyl ether, 20 parts of pure acrylic emulsion, 20 parts of coloring raw materials, defoaming 5 parts of agent, 5 parts of dispersant, 5 parts of preservative, 5 parts of wetting agent, 10 parts of leveling agent, 10 parts of pH regulator;
[0029] S2. Preparation of slurry: first put water, defoamer, dispersant, and preservative into the dispersion tank, and stir it evenly under stirring at a speed of 800r / min, and then add the coloring raw material, wetting agent, and Add it into the dispersion tank, and then disperse it for 30 minutes at a rotating speed of 1400r / min to obtain a slurry;
[0030] S3. Preparation of mixed...
Embodiment 2
[0042] refer to figure 1 , a preparation process of water-based paint, specifically comprising the following steps:
[0043] S1. Select raw materials: select the following components by weight: 320 parts of water, 105 parts of acrylic resin, 155 parts of epoxy resin, 12 parts of fluorescent powder, 22 parts of ethylene glycol, 20 parts of propylene glycol methyl ether, 20 parts of pure acrylic emulsion, 20 parts of coloring raw materials, defoaming 5 parts of agent, 5 parts of dispersant, 5 parts of preservative, 5 parts of wetting agent, 10 parts of leveling agent, 10 parts of pH regulator;
[0044] S2. Preparation of slurry: first put water, defoamer, dispersant, and preservative into the dispersion tank, and stir it evenly under stirring at a speed of 820r / min, and then add the coloring raw material, wetting agent, and Add it into the dispersion tank, and then disperse it for 30 minutes at a rotating speed of 1420r / min to obtain a slurry;
[0045]S3. Prepare mixed interme...
Embodiment 3
[0057] refer to figure 1 , a preparation process of water-based paint, specifically comprising the following steps:
[0058] S1. Select raw materials: select the following components by weight: 380 parts of water, 110 parts of acrylic resin, 160 parts of epoxy resin, 13 parts of fluorescent powder, 25 parts of ethylene glycol, 24 parts of propylene glycol methyl ether, 24 parts of pure acrylic emulsion, 24 parts of coloring raw materials, defoaming 8 parts of agent, 8 parts of dispersant, 5 parts of preservative, 5 parts of wetting agent, 10 parts of leveling agent, 10 parts of pH regulator;
[0059] S2. Preparation of slurry: first put water, defoamer, dispersant, and preservative into the dispersion tank, and stir it evenly under stirring at a speed of 850r / min, and then add the coloring raw material, wetting agent, and Add it into the dispersion tank, and then disperse it for 30 minutes at a rotating speed of 1450r / min to obtain a slurry;
[0060] S3. Prepare mixed interm...