Embodiment 1
[0023] A paper-based insect trap barrier layer and its preparation steps are as follows:
[0024] Step 1: Mix 90 parts of styrene-acrylic latex, 10 parts of styrene-butadiene latex, 5 parts of wax emulsion, and 0.2 parts of defoamer emulsified silicone oil, etc. and mix together mechanically to prepare a composite emulsion. The rotation speed is 300r / min, and the mixing time is 10min.
[0025] Step 2: Add 5 parts of yellow color paste and 1.5 parts of thickener carboxymethyl cellulose, etc. into the composite emulsion prepared in step 1, wherein the rotation speed is preferably 400r / min, and the mixing time is 30min.
[0026] Step 3: Filter the composite emulsion prepared in Step 2, wherein the filter screen is a 325-mesh metal mesh to obtain the barrier layer liquid of the paper-based insect trap.
[0027] Step 4. Use a coating machine to coat the composite emulsion on both sides, wherein the oven temperature is 105°C, and the latex coating amount is 10g / m 2 , to prepare a ...
Embodiment 2
[0029] A paper-based insect trap barrier layer and its preparation steps are as follows:
[0030] Step 1: Mix 50 parts of styrene-acrylic latex, 50 parts of styrene-butadiene latex, 5 parts of wax emulsion, and 0.2 parts of antifoaming agent polyoxypropylene glyceryl ether, etc. and mechanically stir to prepare a composite emulsion, wherein the speed is 300r / min, The mixing time was 10 minutes.
[0031] Step 2: Add 5 parts of yellow color paste and 1 part of thickener guar gum, etc. into the composite emulsion prepared in step 1, wherein the rotation speed is preferably 400r / min, and the mixing time is 30min.
[0032] Step 3: Filter the composite emulsion prepared in Step 2, wherein the filter screen is a 325-mesh metal mesh to obtain the barrier layer liquid of the paper-based insect trap.
[0033] Step 4. Use a coating machine to coat the composite emulsion on both sides, wherein the oven temperature is 105°C, and the latex coating amount is 10g / m 2 , to prepare a waterpro...
Embodiment 3
[0035] A paper-based insect trap barrier layer and its preparation steps are as follows:
[0036] Step 1: Mix 10 parts of styrene-acrylic latex, 90 parts of styrene-butadiene latex, 5 parts of wax emulsion and 0.2 parts of antifoaming agent polydimethylsiloxane, etc. and mechanically stir to prepare a composite emulsion, wherein the rotation speed is 300r / min, the mixing time is 10min.
[0037] Step 2: Add 5 parts of yellow color paste and 2 parts of thickener starch into the composite emulsion prepared in step 1, preferably at a rotation speed of 400r / min, and mixing time of 30 minutes.
[0038] Step 3: Filter the composite emulsion prepared in Step 2, wherein the filter screen is a 325-mesh metal mesh to obtain the barrier layer liquid of the paper-based insect trap.
[0039] Step 4. Use a coating machine to coat the composite emulsion on both sides, wherein the oven temperature is 105°C, and the latex coating amount is 10g / m 2 , to prepare a waterproof paper-based substr...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com