Anticorrosion rust eliminating agent and its preparation method and application
A rust remover and anti-corrosion technology, applied in the field of anti-corrosion and rust remover and its preparation, can solve the problems of boiler, pipeline corrosion, unsafe use, many processes, etc., achieve strong biodegradability, improve production efficiency, simplify The effect of the cleaning process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] Embodiment 1: a kind of anticorrosion derusting agent, component is as follows, is weight percent:
[0031] Ammonium sulfamic acid 60%, ammonium hydrogen fluoride 2.0%, phosphoric acid 30%, edetate disodium 0.5%, calcium hypophosphite 0.05%, hexamethylenetetramine 1.0%, copper sulfate 0.2%, dodecylbenzene Sodium Sulfonate 6.0%, Cocoyl Monoethanolamine 0.25%.
[0032] The preparation method is as follows: weighing the above-mentioned components respectively according to the proportion, adding them in sequence, adding water to prepare a 5.0% solution, and stirring evenly.
Embodiment 2
[0033] Embodiment 2: a kind of anticorrosion derusting agent, component is as follows, is weight percent:
[0034] Sulfamic acid 57%, ammonium hydrogen fluoride 3.0%, phosphoric acid 30%, edetate disodium 1.5%, calcium hypophosphite 0.1%, hexamethylenetetramine 1.05%, copper carbonate 0.15%, dodecylbenzene Sodium Sulfonate 7.0%, Cocoyl Monoethanolamine 0.2%
[0035] The preparation method is as follows: weighing the above-mentioned components respectively according to the proportion, adding water to prepare a 6.0% solution, and stirring until uniform.
Embodiment 3
[0036] Embodiment 3: a kind of anticorrosion derusting agent, component is as follows, is weight percent:
[0037] Ammonium sulfamic acid 60%, ammonium hydrogen fluoride 2.5%, phosphoric acid 25%, disodium edetate 0.8%, calcium hypophosphite 0.35%, hexamethylenetetramine 1.2%, copper sulfate 0.15%, dodecylbenzene Sodium Sulfonate 10%.
[0038] The preparation method is as follows: weighing the above-mentioned components respectively according to the proportion, adding water to prepare a 7.0% solution, and stirring until uniform.