Embodiment 1
[0015] Weigh 100g 2-acrylamido-2-methylpropanesulfonic acid (AMPS), 40g N,N'-dimethylacrylamide (DMAA), 6g acrylic acid (AA), 6g itaconic acid (IA), 0.5g N, N'-methylenebisacrylamide (MBA) was dissolved in 717g of deionized water, and 61g of 40% sodium hydroxide solution was added to adjust the pH value to 6. Add the solution into the reactor, put the reactor into a 60°C constant temperature water bath, pass nitrogen into the reactor to remove oxygen, and after the temperature of the aqueous solution in the reactor reaches 60°C, add 3g of 10% persulfuric acid Potassium solution initiates a reaction, and the reaction lasts for 5 hours to prepare a pentapolymer solution, which is dried and pulverized to obtain an oil well cement fluid loss reducer powder product. The average relative molecular weight of the obtained pentapolymer oil well cement fluid loss reducer is 420,000. Code-named as sample 1.
Embodiment 2
[0017] Weigh 100g 2-acrylamido-2-methylpropanesulfonic acid (AMPS), 60g N,N'-dimethylacrylamide (DMAA), 8g acrylic acid (AA), 8g itaconic acid (IA), 0.3g N, N'-methylenebisacrylamide (MBA), dissolved in 689 g of deionized water. Add 65 g of 40% sodium hydroxide solution to adjust the pH to 6. Add the solution into the reactor, put the reactor into a 60°C constant temperature water bath, pass nitrogen into the reactor to remove oxygen, and after the temperature of the aqueous solution in the reactor reaches 60°C, add 3g of 10% persulfuric acid Potassium solution initiates a reaction, and the reaction lasts for 5 hours to prepare a pentapolymer solution, which is dried and pulverized to obtain an oil well cement fluid loss reducer powder product. The average relative molecular mass of the obtained pentapolymer oil well cement fluid loss reducer is 650,000. Code-named sample 2.
Embodiment 3
[0019] The weight ratio of each component and the operation method of embodiment 3 and embodiment 1 are basically the same, the difference is: 6 g of acrylic acid (AA) in embodiment 1 is replaced by 7.2 g of methacrylic acid. The oil well cement fluid loss reducer (pentapolymer) can also be prepared, and its performance is similar to that of sample 1.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com