Adhesive for artificial boards and preparation method thereof, and plywood prepared from adhesive
A technology for adhesives and wood-based panels, applied in the preparation of adhesives, animal glue or gelatin, adhesive types, etc., can solve the problems of increased production costs, increased product costs, and reduced bonding strength, so as to save production costs and meet water resistance requirements. Requirement, effect of guaranteeing bonding strength
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0051] 1) Prepare materials according to the following weight:
[0052] Demineralized water 70kg
[0054] Defatted Soy Protein Powder 28kg
[0055] Furfuryl alcohol furfural type furan resin 1kg;
[0056] 2) Add sodium carbonate and defatted soybean protein powder into demineralized water in a reaction kettle equipped with a stirrer, thermometer and condensing device, and stir evenly;
[0057] 3) Heat the obtained mixture of sodium carbonate, defatted soybean protein powder and demineralized water to 45-47°C and keep it warm for 3 hours;
[0058] 4) Cool down the mixture obtained in the previous step to 30°C to obtain a uniform soy protein mucus;
[0059] 5) Add furfuryl alcohol furfural furan resin to the soy protein mucus obtained in the previous step, and stir evenly to make a soy protein adhesive for wood-based panels.
[0060] The performance and quality indicators of the obtained adhesive are shown in Table 1.
Embodiment 2
[0062] 1) Prepare materials according to the following weight:
[0063] Demineralized water 65kg
[0064] Sodium carbonate 2kg
[0065] Defatted Soy Protein Powder 30kg
[0066] Furfuryl alcohol furfural type furan resin 3kg;
[0067] 2) Add sodium carbonate and defatted soybean protein powder into demineralized water in a reaction kettle equipped with a stirrer, thermometer and condensing device, and stir evenly;
[0068] 3) Heat the obtained mixture of sodium carbonate, defatted soybean protein powder and demineralized water to 40-42°C and keep it warm for 6 hours;
[0069] 4) Cool down the mixture obtained in the previous step to 30°C to obtain a uniform soy protein mucus;
[0070] 5) Add furfuryl alcohol furfural furan resin to the soy protein mucus obtained in the previous step, and stir evenly to make a soy protein adhesive for wood-based panels.
[0071] The performance and quality indicators of the obtained adhesive are shown in Table 1.
Embodiment 3
[0073] 1) Prepare materials according to the following weight:
[0074] Demineralized water 64kg
[0075] Sodium carbonate 2kg
[0076] Defatted Soy Protein Powder 30kg
[0077] Furfuryl alcohol furfural type furan resin 4kg;
[0078] 2) Add sodium carbonate and defatted soybean protein powder into demineralized water in a reaction kettle equipped with a stirrer, thermometer and condensing device, and stir evenly;
[0079] 3) Heat the obtained mixture of sodium carbonate, defatted soybean protein powder and demineralized water to 68-70°C and keep it warm for 5 hours;
[0080] 4) Cool down the mixture obtained in the previous step to 30°C to obtain a uniform soy protein mucus;
[0081] 5) Add furfuryl alcohol furfural furan resin to the soy protein mucus obtained in the previous step, and stir evenly to make a soy protein adhesive for wood-based panels.
[0082] The performance and quality indicators of the obtained adhesive are shown in Table 1.
[0083] In Table 1, the ...
PUM
Property | Measurement | Unit |
---|---|---|
Bonding strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com