Preparation method and application of polymer retention filter aid containing phenylboronic acid functional group
A retention and drainage aid, phenylboronic acid-functional technology, applied in the field of papermaking, can solve the problems of weak binding force, unable to form stable flocculent precipitates, etc., to achieve low production cost, excellent winding and flocculation effects, and enhanced adhesion ability. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0025] A preparation method of a polymer retention and drainage aid containing phenylboronic acid functional group, the steps are as follows in parts by weight:
[0026] (1) Mixing: Mix 10g of polyvinylamine and 1000mL of water at room temperature, and fully stir to dissolve it; then add 10g of p-carboxyphenylboronic acid to fully dissolve it in the above solution to obtain a mixture;
[0027] (2) Coupling reaction: After 50 minutes, heat up to 40°C, add 0.1M dilute hydrochloric acid to adjust the pH value of the solution to 6.0, and slowly add 1-(3-dimethylaminopropyl)-3-ethyl carbon under the protection of nitrogen 10 g of diimine hydrochloride was stirred for 3 hours, cooled and discharged.
[0028] (3) Separation: Collect the reaction liquid and collect it into the regenerated cellulose dialysis membrane for separation. The separation time is 3 days, and then the solution is dried to a constant weight, and finally a polymer retention and drainage aid containing phenylboron...
Embodiment 2
[0033] A preparation method of a polymer retention and drainage aid containing phenylboronic acid functional group, the steps are as follows in parts by weight:
[0034] (1) Mixing: Mix 10g of polyvinylamine, 1000mL of water and 100mL of ethanol at room temperature, and stir well to dissolve; then add 5g of p-carboxyphenylboronic acid to fully dissolve it in the above solution to obtain a mixture ;
[0035] (2) Coupling reaction: After 90 minutes, heat up to 65°C, add acetic acid to adjust the pH value of the solution to 5.0, and slowly add 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide under nitrogen protection Hydrochloride 18g, stirred for 4h
[0036] After that, cool down and discharge.
[0037] (3) Separation: Collect the reaction liquid and collect it into the regenerated cellulose dialysis membrane for separation. The separation time is 2 days, and then the solution is dried to a constant weight, and finally a polymer retention and drainage aid containing phenylboronic...
Embodiment 3
[0041] A preparation method of a polymer retention and drainage aid containing phenylboronic acid functional group, the steps are as follows in parts by weight:
[0042] (1) Mixing: Mix 10g of polyvinylamine, 800mL of water and 25mL of methanol at room temperature, and fully stir to dissolve it; then add 4g of p-carboxyphenylboronic acid to fully dissolve it in the above solution to obtain a mixture ;
[0043] (2) Coupling reaction: After 60 minutes, heat up to 35°C, add 0.1M oxalic acid to adjust the pH value of the solution to 6.5, slowly add 5g of diisopropylcarbodiimide under nitrogen protection, stir for 2 hours, cool down and discharge; The purpose is to control the initiation of the reaction and reduce the formation of side reactants.
[0044] (3) Separation: Collect the reaction liquid and collect it into the regenerated cellulose dialysis membrane for separation. The separation time is 4 days, and then the solution is dried to a constant weight, and finally a polymer r...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com