A deactivated scr denitrification catalyst regeneration liquid and a regeneration method of deactivated scr denitrification catalyst
A technology for denitration catalyst and regeneration liquid, which is applied in catalyst regeneration/reactivation, chemical instruments and methods, physical/chemical process catalysts, etc. problem, to achieve the effect of improving catalytic activity and improving pore structure
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0058] 1. Preparation of cleaning solution: In the cleaning container device, use deionized water as a solvent, prepare a mixed solution with a molar concentration of sulfuric acid of 0.3mol / L, and a mass fraction of emulsifier sodium lauryl sulfate of 0.05%, and mechanically stir 10min for use.
[0059] 2. Preparation of pore size repair solution: in the pore size repair container device, use deionized water as solvent to prepare a mixed solution with a mass fraction of 5% absolute ethanol and 0.5% polyethylene glycol dispersant, mechanically stir for 10 minutes, and wait for use;
[0060] 3. Preparation of active component replenishment liquid: In the active component replenishment device, use deionized water as solvent to prepare 0.8% ammonium metavanadate, 3.2% tungstinic acid, and 0.1% dodecyl Sodium sulfate emulsifier, 0.5% polyethylene glycol dispersant, adjust the pH value of the solution to 4.5 with oxalic acid or dilute ammonia water, mechanically stir for 30 minute...
Embodiment 2
[0064] 1. Preparation of cleaning solution: In the cleaning container device, use deionized water as a solvent, prepare a mixed solution with a molar concentration of sulfuric acid of 1.0mol / L, and a mass fraction of emulsifier sodium lauryl sulfate of 1%, and mechanically stir 30min for use.
[0065] 2. Preparation of pore size repair solution: In the pore size repair container device, use deionized water as solvent to prepare a mixed solution with a mass fraction of 25% absolute ethanol and 2% polyethylene glycol dispersant, mechanically stir for 30 minutes, and wait for use;
[0066] 3. Preparation of active component replenishment liquid: In the active component replenishment device, use deionized water as a solvent to prepare ammonium metavanadate with a mass fraction of 2.5%, 15% tungstinic acid, and 1% dodecyl Sodium sulfate emulsifier, 1% polyethylene glycol dispersant, adjust the pH value of the solution to about 7 with oxalic acid or dilute ammonia water, mechanical...
Embodiment 3
[0070] 1. Preparation of cleaning solution: In the cleaning container device, use deionized water as a solvent, prepare a mixed solution with a molar concentration of sulfuric acid of 0.5mol / L, and a mass fraction of emulsifier sodium lauryl sulfate of 0.5%, and mechanically stir 20min to be used.
[0071] 2. Preparation of pore size repair solution: In the pore size repair container device, use deionized water as solvent to prepare a mixed solution with a mass fraction of 15% absolute ethanol and 1% polyethylene glycol dispersant, mechanically stir for 20 minutes, and wait for use;
[0072] 3. Preparation of active component replenishment liquid: In the active component replenishment device, use deionized water as a solvent to prepare ammonium metavanadate with a mass fraction of 1.5%, tungstenic acid with 9%, and dodecyl with a mass fraction of 0.5% Sodium sulfate emulsifier, 0.5% polyethylene glycol dispersant, adjust the pH value of the solution to about 5.5 with oxalic a...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com