Self-emulsifying type water curing environment-friendly polyurethane waterproof paint
A polyurethane waterproof and self-emulsifying technology, applied in coatings and other directions, can solve the problems of short operation time, increased production cost, fast reaction speed, etc., and achieve the effects of reducing health hazards, improving mechanical strength, and improving self-emulsification.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] Example 1: Preparation of self-emulsifying water-curable environmentally friendly polyurethane waterproof coating
[0020] Both components A and B are based on 100 parts:
[0021] The specific ratio of component A is: 70 parts of mixed polyether polyol (40 parts of N220, 30 parts of N330), 24 parts of MDI, and 6 parts of plasticizer (diisooctyl phthalate).
[0022] The specific ratio of component B is: 47 parts of liquid filler (37 parts of dibutyl phthalate, 10 parts of chlorinated paraffin), 47 parts of inorganic powder filler (13 parts of light magnesium oxide, 20 parts of light calcium carbonate , 10 parts of talcum powder, 2 parts of anti-settling agent 908, 2 parts of calcium hydroxide), 3 parts of chemical additives (0.5 parts of antifoaming agent polydimethylsiloxane, 0.4 parts of wetting agent, 0.6 parts of dispersing agent, 0.5 part of leveling agent, 1 part of inorganic pigment), 1 part of organic bismuth catalyst, 1 part of dimethylol propionic acid and 1 p...
Embodiment 2
[0027] Example 2: Preparation of self-emulsifying water-curable environmentally friendly polyurethane waterproof coating
[0028] Both components A and B are based on 100 parts:
[0029] The specific proportion of component A is: 60 parts of mixed polyether polyol (30 parts of N220, 30 parts of N330), 30 parts of MDI, and 10 parts of plasticizer (dibutyl phthalate).
[0030] The specific ratio of component B is: 38 parts of liquid filler (38 parts of diisooctyl phthalate), 50 parts of inorganic powder filler (14 parts of light magnesium oxide, 20 parts of light calcium carbonate, 10 parts of talcum powder , 2 parts of anti-settling agent 908, 4 parts of calcium hydroxide), 6 parts of chemical additives (2 parts of antifoaming agent polydimethylsiloxane, 1 part of wetting agent, 1 part of dispersing agent, 1 part of leveling agent , 1 part of inorganic pigment), 0.5 part of organic bismuth catalyst, 0.5 part of dibutyltin dilaurate, 2 parts of dimethylol propionic acid, 2 part...
Embodiment 3
[0035] Example 3: Preparation of self-emulsifying water-curing environment-friendly polyurethane waterproof coating
[0036] Both components A and B are based on 100 parts:
[0037] The specific ratio of component A is: 50 parts of mixed polyether polyol (35 parts of N220, 15 parts of N330), 28 parts of MDI, and 22 parts of plasticizer (diisooctyl phthalate).
[0038] The specific ratio of component B is: 50 parts of liquid filler (10 parts of dibutyl phthalate, 20 parts of chlorinated paraffin and 20 parts of diisooctyl phthalate), 40 parts of inorganic powder filler (15 parts Heavy calcium, 23 parts of talcum powder, 2 parts of anti-settling agent 908,), 5 parts of chemical additives (1 part of antifoaming agent polydimethylsiloxane, 1 part of wetting agent, 1 part of dispersant, 1 part of fluid leveling agent, 1 part inorganic pigment), 1 part organic bismuth catalyst, 2 parts dimethylol propionic acid, 1 part dimethylol butyric acid and 1 part 3-methyl-1,5 pentanediol.
...