A technology for separation and recovery of solutions, applied in chemical instruments and methods, improvement of process efficiency, inorganic chemistry, etc., can solve the problems of complex process, complicated operation, high cost, etc., and achieve short process flow, good separation effect and low production cost low effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0042] Take pH 9.6 containing V25.6g / L, Cr2.3g / L vanadium slag extracting liquid 1.5m 3 , add calcium hydroxide according to 1.3 times of the stoichiometric number of vanadium forming calcium vanadate, stir and ball mill at room temperature for 1.5h, filter to obtain the vanadium-precipitated liquid containing V0.06g / L and the vanadium-enriched slag containing Cr﹤0.1% . The obtained vanadium-precipitated liquid is returned to the vanadium slag extraction and leaching process to continue to use; the obtained vanadium-enriched slag is added with water at a solid-to-liquid ratio of 1:3g / ml, stirred and added with 2mol / LH 2 SO 4 , react at 70°C for 1.5h, control the end point pH value to 3.2, and filter to obtain a vanadium-enriched solution, add ammonium to precipitate vanadium at a mass ratio of ammonium sulfate / vanadium pentoxide to the obtained vanadium-enriched solution, and add sulfuric acid to adjust the pH to 2.0, stirred at 95°C for 1.5h, filtered ammonium polyvanadate,...
Embodiment 2
[0044] Take the obtained solution 1.5m of the vanadium slag calcined sand obtained by liquid leaching after the vanadium precipitation obtained in Example 1 3 , adding calcium oxide according to 1.5 times the stoichiometric number of vanadium forming calcium vanadate, ball milling at 60°C for 1 hour, and filtering to obtain a vanadium-precipitated solution containing V0.02g / L and a vanadium-enriched slag containing Cr﹤0.1%. Add barium carbonate to the vanadium-precipitated solution according to 1.2 times the stoichiometric number of barium chromate formed by the chromium therein, stir and grind at room temperature for 0.5h, filter to obtain the chromium-precipitated solution and chromium-enriched slag containing Cr0.03g / L, and the obtained precipitated The chromium solution is first evaporated and concentrated to 0.5m 3 , and then stirred at room temperature and introduced CO 2 Adjust the pH to 9.2, crystallize and precipitate sodium bicarbonate at 0°C, and return the obtaine...
Embodiment 3
[0046] Take 1500ml of leaching solution obtained from vanadium-chromium reduction slag containing V15.6g / L and Cr28.1g / L with a pH of 10.8, sodium roasting-water leaching, and add calcium oxide according to 1.2 times the stoichiometric number of vanadium forming calcium vanadate , ground for 1 hour at room temperature, and filtered to obtain vanadium-precipitated liquid containing V0.02g / L and vanadium-enriched slag containing Cr﹤0.1%. The obtained vanadium-enriched slag is used to produce vanadium chemical products. The obtained vanadium-precipitated liquid is then added with barium hydroxide according to 1.1 times the stoichiometric number of barium chromate formed by the chromium therein, stirred at room temperature for 0.5h, and filtered to obtain chromium-enriched slag and chrome solution. The obtained chromium-enriched slag is used to produce chromium chemical products; the obtained chromium-precipitated liquid is stirred at room temperature and introduced into 2 Adjust...