[0020] Put 30Kg of industrial grade lard fatty acid, 5Kg of sodium hydroxide and 55kg of water into the reaction kettle, stir at 80°C for 3h, after saponification, add 3Kg of dodecyl betaine, 2Kg of dodecylamine, fatty alcohol poly Oxyethylene ether (AEO-10) 3Kg, Tween-20 2Kg, coconut oil fatty acid diethanolamide (6501) 1Kg and continue to stir until they are evenly mixed.
[0021] The prepared reverse flotation collector is pumped into the phosphate rock slurry stirring tank and mineralized with the ore pulp. The amount added is 0.25Kg / t raw ore. After one flotation, the flotation index of the phosphorous concentrate is P 2 o 5 28.5%, MgO 0.7%, Fe 2 o 3 1.56%, Al 2 o 3 1.65%, P 2 o 5 The recovery rate reaches 87%, which meets the requirement of ore for dihydrate wet-process phosphoric acid production.
Embodiment 2
[0023] Put 30Kg of industrial grade lard fatty acid, 5Kg of sodium hydroxide and 55kg of water into the reaction kettle, stir at 80°C for 3h, after saponification, add 3.5Kg of dodecyl betaine, 1Kg of dodecylamine, Tween -20 2Kg, fatty alcohol polyoxyethylene ether (AEO-10) 3Kg, coconut oil fatty acid diethanolamide (6501) 1Kg and continue to stir until evenly mixed.
[0024] The prepared reverse flotation collector is pumped into the phosphate rock slurry stirring tank and mineralized with the ore pulp. The amount added is 0.25Kg / t raw ore. After one flotation, the flotation index of the phosphorous concentrate is P 2 o 5 28.5%, MgO 0.7%, Fe 2 o 3 1.56%, Al 2 o 3 1.65%, P 2 o 5 The recovery rate reaches 87%, which meets the requirement of ore for dihydrate wet-process phosphoric acid production.
Embodiment 3
[0026] Put 35Kg of industrial grade tallow fatty acid, 8Kg of sodium bicarbonate and 42Kg of water into the reaction kettle, stir at 80°C for 3h, after saponification, add 4Kg of lauryl betaine, 2Kg of octadecylamine, Tween-40 3Kg, 4Kg of fatty alcohol polyoxyethylene ether (AEO-15), and 2Kg of sodium dodecylbenzenesulfonate continue to stir until they are evenly mixed.
[0027] The prepared reverse flotation collector is pumped into the phosphate slurry stirring tank and the slurry is mineralized. The addition amount is 0.3Kg / t raw ore. After one flotation, the flotation index of the phosphorus concentrate is P 2 o 5 29.3%, MgO 0.68%, Fe 2 o 3 1.49%, Al 2 o 3 1.55%, P 2 o 5 The recovery rate reaches 85%, meeting the requirement of dihydrate wet-process phosphoric acid production ore.