Colorful environment-friendly dust suppressant and preparation and use methods thereof
A dust suppressant and environmental protection technology, applied in the field of environmental protection and dust suppression, to achieve the effect of improving dust suppression effect, increasing penetration, and facilitating differentiated management
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0025] Colorful environmental dust suppressant, composed of the following components by weight percentage: 3.5% hydroxypropyl cellulose modified cellulose, 3.0% carboxymethyl cellulose, 0.3% pure acrylic emulsion, 0.2% polyoxyethylene alkylphenol ether , 3% ethylene glycol, 2% glycerin, 8% pigments and fillers (select titanium nickel yellow and bentonite to mix at a ratio of 3:1), 0.4% benzotriazole, and the balance is water.
[0026] Preparation methods include:
[0027] Step 1: Add water, 3.5% hydroxypropyl cellulose modified cellulose, 3.0% carboxymethyl cellulose, 8% pigments and fillers (select titanium nickel yellow and bentonite to mix at a ratio of 3:1) to the container at 1200rpm / min stirring for 12 min;
[0028] Step 2: Reduce the stirring speed to 400rpm / min, add 0.3% pure acrylic emulsion, 0.2% polyoxyethylene alkylphenol ether, 3% ethylene glycol, 2% glycerin, 0.4% styrene-acrylic acid to the solution in step 1 Triazole, stirred for 10 minutes, that is, a color...
Embodiment 2
[0030] Colorful environment-friendly dust suppressant, composed of the following components by weight percentage: 10% carboxymethyl cellulose, 1.3% styrene-acrylic emulsion, 2.0% EVA emulsion, 0.05% sodium dodecylsulfonate, 0.05% polyoxyethylene fat Alcohol ether, 8% polyethylene glycol, 4% ethylene glycol, 10% pigments and fillers (choose iron oxide brown and high clay mixed at a ratio of 1.2:1), 0.2% benzotriazole, 0.3% borax, the balance for water.
[0031] Preparation methods include:
[0032] Step 1: Add water, 10% carboxymethyl cellulose, 10% pigments and fillers (choose brown iron oxide and high clay to mix at a ratio of 1.2:1) into the container and stir at 1000rpm / min for 10min;
[0033] Step 2: Reduce the stirring speed to 380rpm / min, add 1.3% styrene-acrylic emulsion, 2.0% EVA emulsion, 0.05% sodium dodecylsulfonate, 0.05% polyoxyethylene fatty alcohol ether, 8% Polyethylene glycol, 4% ethylene glycol, 0.2% benzotriazole, 0.3% borax, stirred for 10 minutes, that i...
Embodiment 3
[0035] Colorful environmental dust suppressant, composed of the following components by weight percentage: 1.0% methyl cellulose, 5.6% carboxymethyl hydroxyethyl cellulose, 0.1% silicon acrylic emulsion, 0.5% styrene acrylic emulsion, 0.15% sodium polyacrylate , 0.01% sodium dodecylbenzene sulfonate, 0.24% polyethylene glycol, 6.4% ethylene glycol, 15% pigments and fillers (select iron oxide green, calcium carbonate, attapulgite to mix in a ratio of 1.7:1:1) , 0.3% benzotriazole, 0.1% borax, and the balance is water.
[0036] Preparation methods include:
[0037] Step 1: Add water, 1.0% methyl cellulose, 5.6% carboxymethyl hydroxyethyl cellulose, 15% pigments and fillers to the container (choose iron oxide green, calcium carbonate, attapulgite at a ratio of 1.7:1:1 Mixing) stirring at 1500rpm / min for 10min;
[0038] Step 2: Reduce the stirring speed to 350rpm / min, add 0.1% silicon acrylic emulsion, 0.5% styrene acrylic emulsion, 0.15% sodium polyacrylate, 0.01% sodium dodecy...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com