Preparation method of cellulose toughened silica airgel

A technology of silica and cellulose, which is applied in the field of airgel, can solve the problems of expensive production equipment and production costs, damage to the skeleton structure of airgel, difficulty in continuous large-scale production, etc., and achieve reduced synthesis steps and high hydrophobicity and mechanical properties, the effect of enhancing structural strength

Active Publication Date: 2020-08-28
CHANGCHUN UNIV OF TECH
View PDF5 Cites 1 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

Although the airgel prepared by this method has good flexibility, the supercritical drying method used in the drying process requires high-pressure equipment, high energy consumption for the process, very expensive production equipment and production costs, and strict control of process conditions. It is dangerous, and the whole drying process takes a long time, and it is difficult to achieve continuous large-scale production, thus limiting its development to a large extent
[0005] Material composite method is an important method to improve the strength and toughness of silica aerogels. The most widely used methods include additive method, fiber reinforcement method, secondary composite method and polymer method. Among them, the fiber reinforcement method has the characteristics of simple operation, but Inorganic fibers can improve the mechanical properties of aerogels, but doping them into aerogels will destroy the skeleton structure of aerogels to a certain extent

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0018] The preparation method of cellulose toughened silica airgel, comprises the following steps:

[0019] Step 1: Preparation of cellulose sol: according to the ratio of 1g:20mL, immerse the cotton raw material in 98% concentrated sulfuric acid solution, soak for 30min, stir in a water bath at 60°C for 2h, and then rinse the obtained cellulose solution with deionized water And centrifuged 15 times, the solution is close to neutral, the deionized water is pumped out, and the rest is cellulose sol;

[0020] Step 2: The components methyltrimethoxysilane, dimethyldimethoxysilane, hexadecyltrimethylammonium bromide, N,N-dimethylamide, CH 3 COOH (mass fraction 0.1%), CH 3 CH 2 OH was mixed uniformly according to the ratio of 1mL: 0.8mL: 0.3g: 0.8mL: 9mL: 6mL, and then stirred in a water bath at 30°C for 60min to obtain the base liquid;

[0021] Step 3: Add pre-prepared cellulose sol to the base liquid obtained in step 2 according to the ratio of base liquid volume and cellulose...

Embodiment 2

[0024] The preparation method of cellulose toughened silica airgel, comprises the following steps:

[0025] Step 1: Preparation of cellulose sol: according to the ratio of 1g:25mL, immerse the cotton raw material in concentrated sulfuric acid solution, soak for 25min, stir in a water bath at 50°C for 3h, then rinse the obtained cellulose solution with deionized water and centrifuge Several times, until the solution is close to neutral, the deionized water is pumped out, and the rest is cellulose sol;

[0026] Step 2: The components methyltrimethoxysilane, dimethyldimethoxysilane, hexadecyltrimethylammonium bromide, N,N-dimethylamide, CH 3 COOH (mass fraction 0.1%), CH 3 CH 2 OH was mixed uniformly according to the ratio of 1mL: 0.5mL: 0.15g: 0.5mL: 12mL: 8mL, and then stirred in a water bath at 40°C for 80min to obtain the base liquid;

[0027] Step 3: Add pre-prepared cellulose sol to the base liquid obtained in step 2 according to the ratio of base liquid volume and cellu...

Embodiment 3

[0030] The preparation method of cellulose toughened silica airgel, comprises the following steps:

[0031] Step 1: Preparation of cellulose sol: according to the ratio of 1g:30mL, immerse the cotton raw material in 98% concentrated sulfuric acid solution, soak for 35min, stir in a water bath at 60°C for 3h, and then rinse the obtained cellulose solution with deionized water And centrifuge several times until the solution is close to neutral, then remove the deionized water, and the rest is cellulose sol;

[0032] Step 2: The components methyltrimethoxysilane, dimethyldimethoxysilane, hexadecyltrimethylammonium bromide, N,N-dimethylamide, CH 3 COOH (mass fraction 0.1%), CH 3 CH 2 OH was mixed uniformly according to the ratio of 1mL: 0.8mL: 0.25g: 0.7mL: 15mL: 10mL, and then stirred in a water bath at 30°C for 60min to obtain the base liquid;

[0033] Step 3: Add pre-prepared cellulose sol to the base liquid obtained in step 2 according to the ratio of base liquid volume and...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

A preparation method of cellulose-toughened silicon dioxide aerogel includes following steps: (1), according to a proportion of 1g:(15-30)mL, soaking cotton in concentrated sulfuric acid for 20-35min,stirring at 40-60 DEG C for 2-3h, using deionized water to flush, centrifuging for several times until a solution is close to neutral, and extracting the deionized water to obtain cellulose sol; (2),mixing methyl trimethoxy silane, dimethyl dimethoxy silane, cetyl trimethyl ammonium bromide, N, N-dimethylformamide, CH3COOH and CH3CH2OH according to a proportion of 1mL:(0.4-0.9)mL:(0.1-0.3)g:(0.4-0.8)mL:(8-20)mL:(5-10)mL, and stirring at 25-40 DEG C for 60-80min; (3), adding the cellulose sol into mixed liquid according to a proportion of 1mL:(0.5-4.0)g, using ammonia water to adjust pH to 8-9, and aging at 35-50 DEG C for 5-8h; (4), using isopropanol and n-hexane for washing, drying at 30-35 DEG C for 10-15h, and drying at 38-45 DEG C for 20-40h to obtain the cellulose-toughened silicondioxide aerogel. The aerogel is high in porosity, hydrophobicity, mechanical performance and oil absorption rate and reusable.

Description

technical field [0001] The invention belongs to the field of airgel, and in particular relates to a preparation method of cellulose toughened silica airgel. Background technique [0002] Silica airgel is a new type of amorphous solid porous material composed of nano-sized particles and air as the dispersion medium. Due to its low density, high porosity, high specific surface area, low thermal conductivity, low acoustic wave With a series of characteristics such as propagation rate and low dielectric constant, it is a kind of nanoporous lightweight material with high specific surface area and excellent adsorption performance, and has broad application prospects in the fields of environmental protection and energy utilization. [0003] Since the traditional SiO prepared from tetraethyl orthosilicate as precursor 2 The surface of airgel is connected with hydrophilic group -OH, and has a porous structure, which will lead to SiO 2 Airgel readily absorbs moisture. The re-evapor...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Patents(China)
IPC IPC(8): C04B30/02C01B33/157
CPCC01B33/1585C04B30/02C04B18/248
Inventor 李贞玉贾菲胡明忠刘雪雁张竹青王桃施晨
Owner CHANGCHUN UNIV OF TECH
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products