[0031] (1) Preparation of inhibitors: Weigh 1 gram of cocamidopropyl betaine, 1 gram of trimercaptotriazine trisodium salt and 1 gram of dextrin and add them to 30° C. water for dissolution, and stir at room temperature for 3 hours to obtain 3 g of mixed solution of separation flotation inhibitor.
[0032] (2) The prepared separation flotation inhibitor is carried out to the actual mineral flotation experiment:
[0033] Firstly, the raw ore containing copper and molybdenum is subjected to flotation to obtain copper-molybdenum mixed concentrate, and then the obtained copper-molybdenum mixed concentrate is directly subjected to separation and flotation experiments.
[0034] After phase and composition analysis, the molybdenum minerals in the copper-molybdenum mixed concentrate mainly exist in the form of molybdenite, and the copper minerals mainly exist in the form of chalcopyrite, and lubricating oil and talc components are detected on the surface of the minerals and contain ab...
Embodiment 2
[0042] (1) Preparation of inhibitors: Weigh 1 gram of cocamidopropyl betaine, 3 grams of trimercaptotriazine trisodium salt and 0.5 gram of carboxymethyl cellulose and add them to 50° C. water for dissolving. Stir for 12 hours to obtain a mixed solution containing 4.5 g of separation flotation inhibitor.
[0043] (2) the prepared separation flotation inhibitor is carried out to the actual mineral flotation experiment:
[0044] First, the raw ore containing lead and molybdenum is subjected to flotation to obtain a lead-molybdenum mixed concentrate, and then the obtained lead-molybdenum mixed concentrate is directly subjected to a separation flotation experiment.
[0045] After phase and composition analysis, the molybdenum minerals in the lead-molybdenum mixed concentrate mainly exist in the form of molybdenite, the lead minerals mainly exist in the form of galena, and the lead-molybdenum mixed concentrate also contains pyrite and sphalerite , argillaceous minerals were detect...
Embodiment 3
[0053] (1) Preparation of inhibitors: Weigh 1 gram of cocamidopropyl betaine, 0.5 gram of trimercaptotriazine trisodium salt and 0.1 gram of gull gum and dissolve them in 70°C water, and stir at 70°C for 20 hours A mixed solution containing 1.6 g of separation flotation inhibitor was obtained.
[0054] (2) the prepared separation flotation inhibitor is carried out to the actual mineral flotation experiment:
[0055] Firstly, the raw ore containing molybdenum and bismuth is subjected to flotation to obtain a molybdenum-bismuth mixed concentrate, and then the obtained molybdenum-bismuth mixed concentrate is directly subjected to a separation flotation experiment.
[0056] According to phase and composition analysis, the molybdenum minerals in the molybdenum-bismuth mixed concentrate mainly exist in the form of molybdenite, and the bismuth minerals mainly exist in the form of bismuthite. The molybdenum-bismuth mixed concentrate also contains pyrite, chalcopyrite and Sphalerite, ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com