A kind of dendrobium polysaccharide nanocellulose hydrogel
A technology of nanocellulose and dendrobium polysaccharides, which is applied in the field of hydrogel materials and skin care products, can solve the problems of restricting the promotion and application of skin care products, the reduction of skin care effects, and poor thermal stability, so as to delay skin aging and tighten skin Good effect on aging and thermal stability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0046] Prepare modified nanocellulose, comprising the following steps:
[0047] Step 1: Put 8 g of cellulose and 2 g of carboxymethyl cellulose into 40 ml of a mixed solvent and stir and mix them for 20 min at a speed of 300 r / min at a temperature of 20° C. to form the first mixed solution; (wherein the mixed solvent It is a mixture of acetone and N,N-dimethylacetamide, the volume ratio is 2:1)
[0048] Step 2: Add 1g modifier to the first mixed solution and stir and mix, and mix for 10 minutes at a speed of 400r / min and a temperature of 20°C to form a second mixed solution; then use 0.01M aqueous sodium hydroxide solution The pH of the second mixed solution was adjusted to 10-11, and at the same time, the temperature of the second mixed solution was raised to 60° C. for modification treatment, and the modification time was 3 hours, thereby preparing modified nanocellulose.
[0049] The modifiers are 3-[2-(pentafluorohexyl)ethoxy]-1,2-cycloethoxypropane, 5-chloro-1-(4-piperid...
Embodiment 2
[0051] The preparation of dendrobium polysaccharide nanocellulose hydrogel comprises the following steps:
[0052] Step 1: Place 2.5g of modified nanocellulose (prepared by Example 1), 0.9g of dendrobium polysaccharide and 0.3g of regulator in 20ml of deionized water, stir and mix, and mix well to form a mixed solution;
[0053] Step 2: Add 0.06g N-hydroxysuccinimide and 0.04g 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide to the mixture, stir and mix for 15 minutes, then add 0.5 g of polyvinyl alcohol and 0.1 g of a crosslinking agent were reacted at a temperature of 70°C for a reaction time of 4 hours to prepare a hydrogel.
[0054] The regulator is 3-mercaptopropionic acid-2-ethyl-2-[(3-mercapto-1-oxopropoxyl)methyl]-1,3-propylene diester, N-bromobutane A mixture of imide and 1,2-epoxy-4-vinylcyclohexane in a mass ratio of 1:2:2.
[0055] The crosslinking agent is a mixture of glutaraldehyde and diglycolic anhydride, and its mass ratio is 4:1.
Embodiment 3
[0057]An essence containing dendrobium polysaccharide nanocellulose hydrogel, the preparation method of which comprises the following steps:
[0058] Step 1: Add 0.4g glycerin, 0.3g propylene glycol, 0.1g sodium hyaluronate, 0.1g mannitol, 0.1g glutathione and 0.1g sodium polyglutamate into 20ml deionized water and stir to mix. Mix at 200rpm and 15°C for 30min to form the third mixed liquid;
[0059] Step 2: Then 3g dendrobium polysaccharide nanocellulose hydrogel (made by embodiment 2), 0.4g xanthan gum, 0.1g pearl powder and 0.2g rose essential oil are added successively in the third mixed solution and stirred and mixed. Mix at 400 rpm and 15°C for 90 minutes to prepare essence lotion.