Embodiment 1
[0022] Select 200kg of sand, 75kg of ordinary portland cement, 10kg of sulphoaluminate cement, 7kg of silica fume, 12kg of fly ash, 0.22kg of water reducing agent, 2kg of toughening agent, 0.05kg of water retaining agent, 1.5kg of expansion agent, polypropylene Fiber 0.15kg. Add the above components in sequence in the mixer, and mix well to make high-performance mortar 1. Mix mortar 1 with 29 parts of water to obtain product 1, the properties are as follows:
[0023] Jump table fluidity (mm) 167
[0024] 1d compressive / flexural strength (MPa) 20.5 / 4.7
[0025] 28d compressive / flexural strength (MPa) 69.8 / 13.3
[0026] 28d bonding strength (MPa) 2.8
[0027] 28d folding ratio 5.2
[0028] 60d shrinkage rate 390×10 -6
Embodiment 2
[0030] Select 200kg of sand, 65kg of ordinary portland cement, 20kg of sulphoaluminate cement, 5kg of silica fume, 10kg of fly ash, 0.2kg of water reducing agent, 3kg of toughening agent, 0.06kg of water retaining agent, 2.0kg of expansion agent, polyethylene Alcohol fiber 0.1kg. Add the above components in sequence in the mixer, and mix well to make high-performance mortar 2. Mix mortar 2 with 29 parts of water to obtain product 2, the properties are as follows:
[0031] Jump table fluidity (mm) 170
[0032] 1d compressive / flexural strength (MPa) 24.6 / 5.8
[0033] 28d compressive / flexural strength (MPa) 65.4 / 14.0
[0034] 28d bonding strength (MPa) 3.1
[0035] 28d folding ratio 4.7
[0036] 60d shrinkage rate 362×10 -6
Embodiment 3
[0038] Select 200kg of sand, 55kg of ordinary portland cement, 30kg of sulphoaluminate cement, 3kg of silica fume, 8kg of fly ash, 0.18kg of water reducing agent, 4kg of toughening agent, 0.04kg of water retaining agent, 1.0kg of expansion agent, polypropylene Fiber 0.2kg. Add the above components in sequence in the mixer, and mix well to make high-performance mortar 3. Mixing mortar 3 with 29 parts of water to obtain product 3, the product properties are as follows:
[0039] Jump table fluidity (mm) 165
[0040] 1d compressive / flexural strength (MPa) 26.2 / 5.8
[0041] 28d compressive / flexural strength (MPa) 60.7 / 13.6
[0042] 28d bonding strength (MPa) 3.3
[0043] 28d folding ratio 4.5
[0044] 60d shrinkage rate 330×10 -6
PUM
Property | Measurement | Unit |
---|---|---|
shrinkage | aaaaa | aaaaa |
shrinkage | aaaaa | aaaaa |
shrinkage | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com