Energy-saving marble-imitating paint preparation method and product thereof
A technology of imitating marble paint and slurry, which is applied in the field of preparation of energy-saving imitating marble paint, can solve the problems of inconsistent colors, heavy weight of natural stone, complex construction technology, etc., and achieve rich texture texture, low weight, and simple preparation process Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0083] Embodiment 1: a kind of energy-saving imitation marble coating preparation method that the present embodiment provides, it comprises the following steps:
[0084] (1) Preparation of silicate slurry: the components and weight percentages of the raw materials of the silicate slurry are as follows:
[0085] Water 85-95%,
[0086] TSPP 0.4-1%,
[0087] Sheet silicate 4-14%,
[0088] Add water into the mixing tank, start the mixing tank to stir and disperse, add TSPP and sheet silicate in sequence, and then stir evenly to prepare silicate slurry;
[0089] (2) Preparation of white latex paint: the components and weight percentages of the raw materials of white latex paint are as follows:
[0090] Water 30-40%,
[0091] Hydroxyethylcellulose 0.5-1%,
[0092] Dispersant 0.3-0.8%,
[0093] Wetting agent 0.2-0.5%,
[0094] PH regulator 0.1-0.2%,
[0095] The first part of defoamer 0.1-0.4%,
[0096] Titanium dioxide 1-3%,
[0097] Heavy calcium 4-6%,
[0098] Kaolin 8-...
Embodiment 2
[0166] Embodiment 2: the goods that a kind of above-mentioned energy-saving imitation marble coating preparation method makes, its each component and weight percentage thereof are as follows:
[0167] Silicate slurry 20%,
[0168] A, B, C color paint 40%,
[0169] Thickener 0.4%,
[0170] water 20%,
[0171] The second pure acrylic emulsion 18.5%,
[0172] TEXANOL 1%,
[0173] The third part of defoamer 0.1%,
[0174] Wherein each component of silicate slurry and percentage by weight thereof are as follows:
[0175] Water 85%,
[0176] TSPP 1%,
[0177] Sheet silicate 14%,
[0178] The A, B, and C colored paints are formed by adding A, B, and C colored paints to the white latex paint, wherein the components and weight percentages of the white latex paint are as follows:
[0179] water 30%,
[0180] Hydroxyethyl Cellulose 1%,
[0181] Dispersant 0.8%,
[0182] Wetting agent 0.2%,
[0183] PH regulator 0.2%,
[0184] The first part of defoamer 0.4%,
[0185] Titan...
Embodiment 3
[0194] Embodiment 3: It differs from Embodiment 2 in that the components in the product and their weight percentages are different. Its each component and weight percentage thereof are as follows:
[0195] Its each component and weight percentage thereof are as follows:
[0196] Silicate slurry 30%,
[0197] A, B, C color paint 36.9%,
[0198] Thickener 0.8%,
[0199] water 10%,
[0200] The second pure acrylic emulsion 20%,
[0201] TEXANOL 2%,
[0202] The third part of defoamer 0.3%,
[0203] Wherein each component of silicate slurry and percentage by weight thereof are as follows:
[0204] Water 95%,
[0205] TSPP 1%,
[0206] Sheet silicate 4%,
[0207] The A, B, and C colored paints are formed by adding A, B, and C colored paints to the white latex paint, wherein the components and weight percentages of the white latex paint are as follows:
[0208] water 40%,
[0209] Hydroxyethylcellulose 0.5%,
[0210] Dispersant 0.3%,
[0211] Wetting agent 0.5%,
[0212...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com