A kind of application method of lime mud in papermaking filling
An application method and technology of lime mud, applied in the field of pulp and paper making, can solve the problems of inability to reduce the adverse effects of filling, complex process operation, high production cost, etc., and achieve the goal of improving lime mud retention rate, simple process and low production cost Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0023] (1) Add 2g (absolutely dry) plant fiber raw material (mass ratio of chemical mechanical pulp: chemical reed pulp: bleached kraft softwood pulp = 4:3:3) into 1500ml of water, and use a decomposer to decompose at 5000 rpm.
[0024] (2) Add 31.5% (based on the absolute dry mass of plant fiber raw material) white mud, 0.75% (based on the absolute dry mass of plant fiber raw material) cationic starch, 0.25% (based on the absolute dry mass of plant fiber raw material) in the slurry that step (1) obtains successively The absolute dry mass of the fiber raw material) AKD, 0.04% (based on the absolute dry mass of the plant fiber raw material) cationic polyacrylamide, after stirring evenly, copy the slices on a fast slicer.
[0025] (3) After equilibrating the moisture in the hand-sheet obtained in (2) for 24 hours under the conditions of (23±1)°C and (50±2)% relative humidity, according to GB / T 1540-2002, GB / T 12914- 2008, GB / T 454-2002, GB / T 455-2002 and GB / T22877-2008 Determina...
Embodiment 2
[0035] (1) Add 2g (absolutely dry) plant fiber raw material (mass ratio of chemical mechanical pulp: chemical reed pulp: bleached kraft softwood pulp = 4:3:3) into 1500ml of water, and use a decomposer to decompose at 5000 rpm.
[0036] (2) in the slurry that step (1) obtains successively, add 39% (based on the dry mass of plant fiber raw material) white mud, 0.75% (based on the dry mass of plant fiber raw material) cationic starch, 0.25% (based on the dry mass of plant fiber raw material) The absolute dry mass of the fiber raw material) AKD, 0.04% (based on the absolute dry mass of the plant fiber raw material) cationic polyacrylamide, after stirring evenly, copy the slices on a fast slicer.
[0037] (3) After equilibrating the moisture in the hand-sheet obtained in (2) for 24 hours under the conditions of (23±1)°C and (50±2)% relative humidity, according to GB / T 1540-2002, GB / T 12914- 2008, GB / T 454-2002, GB / T 455-2002 and GB / T22877-2008 Determination of paper Cobb value, te...
Embodiment 3
[0047] (1) Add 2g (absolutely dry) plant fiber raw material (mass ratio of chemical mechanical pulp: chemical reed pulp: bleached kraft softwood pulp = 4:3:3) into 1500ml of water, and use a decomposer to decompose at 5000 rpm.
[0048] (2) Disperse 19% (based on the absolute dry mass of the plant fiber raw material) lime mud in water to form a suspension with a mass fraction of 1%. Then add 0.04% (based on the dry mass of the plant fiber raw material) cationic polyacrylamide, 0.75% (based on the dry mass of the plant fiber raw material) cationic starch, and 0.25% (based on the dry mass of the plant fiber raw material) AKD. Stir with a magnetic stirrer at a speed of 600 rpm for 10 min to obtain a white mud floc suspension.
[0049] (3) Pour the white mud floc suspension obtained in the step (2) into the slurry obtained in the step (1), stir it evenly, and then use a quick slicer to slice.
[0050] (4) After equilibrating the moisture in the hand-sheet obtained in step (3) for...