A heat-resistant jelly
A gel and temperature-resistant technology, which is applied in the field of acrylamide/acryloyloxyethyltrimethylammonium chloride temperature-resistant gel and polymer plugging agent, can solve the problem of non-selective plugging, poor operability, and poor construction Difficulty and other issues, to achieve excellent injection performance, excellent temperature resistance, and the effect of inhibiting syneresis
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0025] Add 0.2g sodium tripolyphosphate, 0.05g paraformaldehyde, 0.05g phenol, 0.3g thiourea, 0.1g sodium malonate to 50g tap water, stir evenly to make it fully dissolved, then add 50g tap water to prepare the mass The acrylamide / acryloxyethyltrimethylammonium chloride with a concentration of 0.8% is mixed with the above solution and stirred evenly to obtain the gelling solution of the present invention. The gelling time of the gelling solution was 39 hours at 160° C., and the strength of the obtained jelly was 0.083 MPa. There was no dehydration phenomenon after aging at 160° C. for 180 days.
Embodiment 2
[0027] Add 0.2g sodium tripolyphosphate, 0.05g sodium aminomethylene phosphonate, 0.05g paraformaldehyde, 0.08g phenol, 0.3g thiourea, 0.1g sodium malonate to 50g of 2% NaCl aqueous solution, stir well , make it fully dissolved, then mix 50g of acrylamide / acryloyloxyethyltrimethylammonium chloride with a mass concentration of 0.8% prepared with tap water with the above solution, and stir evenly to obtain the gelling solution of the present invention. The gelling time of the gelling solution was 36 hours at 160° C., and the strength of the obtained jelly was 0.088 MPa, and there was no dehydration phenomenon after aging at 160° C. for 180 days.
Embodiment 3
[0029] Add 0.3g sodium tripolyphosphate, 0.1g sodium aminomethylene phosphonate, 0.06g paraformaldehyde, 0.1g phenol, 0.3g thiourea, 0.1g sodium malonate to 50g of 6% NaCl aqueous solution, stir well , make it fully dissolved, then mix 50g of acrylamide / acryloyloxyethyltrimethylammonium chloride with a mass concentration of 1% prepared with tap water with the above solution, and stir evenly to obtain the gelling solution of the present invention. The gelling time of the gelling solution is 30 hours at 160° C., the strength of the obtained jelly is 0.089 MPa, and there is no dehydration phenomenon after aging at 160° C. for 180 days.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com