A biodegradable modified urea-formaldehyde resin adhesive and its application
A urea-formaldehyde resin glue, biodegradable technology, used in adhesives, aldehyde/ketone condensation polymer adhesives, adhesive types, etc., can solve problems such as reducing formaldehyde emission
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0025] Example 1 Preparation of degradable modified urea-formaldehyde resin
[0026] (a) Add 702g of water into the reaction kettle, then add 0.4g of KOH, heat to 70°C, add 105g of soybean protein isolate while stirring at a speed of 400rpm, then heat up to 80°C and keep warm for 1 hour to obtain a protein hydrolyzate, then cooled to 25°C;
[0027] (b) Add 117g urea to the reaction kettle, stir and mix evenly, add formaldehyde solution, adjust pH to 8.0 with KOH solution with a mass fraction of 20% at 25-30°C, then heat up to 60°C, add 87g urea again , heat up to 90°C, and keep it for 0.5h; slowly adjust the pH of the reaction solution to 4.5 with a mass fraction of 20% phosphoric acid solution, and continue to keep the temperature at 90°C until the reaction droplets are dropped into 25-28°C clear water, after seeing white clouds, That is, the reaction is ended; the pH of the reaction solution is adjusted to 7.8 with KOH solution, then the temperature of the reaction solution...
Embodiment 2
[0033] (a) Add 480g of water into the reactor, add 1.1g of potassium hydroxide, start heating, when heated to 70°C, while stirring rapidly, add 72g of soybean protein isolate, heat to 80°C, and keep warm for 1 h to obtain protein hydrolyzate.
[0034] Step b and step c are the same as in Example 1.
[0035] (d) Mix the block copolymer obtained in step b and the protein hydrolyzate obtained in step c uniformly at a mass ratio of 1:0.1 to obtain a biodegradable modified urea-formaldehyde resin adhesive
Embodiment 3
[0037] (a) Add 326g of water into the reaction kettle, add 1.3g of potassium hydroxide, start heating, after heating to 70°C, while stirring rapidly, add 48g of soybean protein isolate, and heat to 80°C for 1 hour.
[0038] Step b and step c are the same as in Example 1.
[0039] (d) Mixing the block copolymer obtained in step b and the protein hydrolyzate obtained in step c uniformly at a mass ratio of 1:0.3, to obtain a biodegradable modified urea-formaldehyde resin adhesive.
PUM
Property | Measurement | Unit |
---|---|---|
Ash content | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com