A kind of preparation method of the reticular polyurethane microbial carrier adding modified montmorillonite
A microbial carrier, montmorillonite technology, which is applied in the treatment of granular microbial carriers, chemical instruments and methods, biological water/sewage treatment, etc. The problem of slow film hanging speed, etc., achieves the effect of good bioaffinity, improved nitrification reaction rate, and fast film hanging speed.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] The preparation method of the reticular polyurethane microbial carrier that adds modified montmorillonite of the present embodiment may further comprise the steps:
[0031] Step 1: 10 parts of vinyl polyoxypropylene polyol vinyl polyethylene oxide polyol, 80 parts of ethylene glycol polyether polyol, H 2 Add 5 parts of O, 1 part of silicone oil, 0.1 part of tin catalyst stannous octoate, 0.3 part of amine catalyst triethylenediamine, and 20 parts of olefin monomer styrene into the reaction kettle, stir evenly; add 0.2 part of modified montmorillonite , stirred evenly, and kept warm to 40 ° C, as component 1; the above-mentioned parts are parts by mass;
[0032] Step 2: Add 125 parts of diphenylmethane diisocyanate (MDI) and 0.08 part of free radical polymerization initiator benzoyl peroxide (BPO) into the reactor, stir evenly, and use it as component 2; the above-mentioned parts are parts by mass ;
[0033] Step 3: Mix component 1 and component 2, stir evenly, pour in...
Embodiment 2
[0036] The preparation method of the reticular polyurethane microbial carrier that adds modified montmorillonite of the present embodiment may further comprise the steps:
[0037] Step 1: 15 parts of vinyl polyethylene oxide polyol, 100 parts of ethylene glycol tetrahydrofuran polyether polyol, 10 parts of adipic acid polyester polyol, H 2 Add 6 parts of O, 2 parts of silicone oil, 0.15 parts of tin catalyst stannous octoate, 0.5 parts of amine catalyst triethylenediamine, and 15 parts of olefin monomer styrene into the reaction kettle, stir evenly; add 0.5 parts of modified montmorillonite , stirred evenly, and kept warm to 40 ° C, as component 1; the above-mentioned parts are parts by mass;
[0038] Step 2: Add 130 parts of diphenylmethane diisocyanate (MDI) and 0.06 parts of free radical polymerization initiator azobisisobutyronitrile into the reaction kettle, stir evenly, and use it as component 2; the above-mentioned parts are parts by mass;
[0039] Step 3: Mix componen...
Embodiment 3
[0042] The preparation method of the reticular polyurethane microbial carrier that adds modified montmorillonite of the present embodiment may further comprise the steps:
[0043] Step 1: 5 parts of vinyl polyethylene oxide polyol, 70 parts of oxypropylene polyether polyol, 30 parts of aromatic polyester polyol, H 2 8 parts of O, 2 parts of silicone oil, 0.05 part of tin catalyst dibutyltin dilaurate, 0.8 part of amine catalyst triethylamine, and 5 parts of olefin monomer divinylbenzene were added to the reaction kettle, and stirred evenly; Active montmorillonite, stirred evenly, and kept warm to 35 ° C, as component 1; the above-mentioned parts are parts by mass;
[0044] Step 2: Add 120 parts of diphenylmethane diisocyanate (MDI) and 0.01 part of free radical polymerization initiator benzoyl peroxide (BPO) into the reactor, stir evenly, as component 2; the above-mentioned parts are parts by mass ;
[0045] Step 3: Mix component 1 and component 2, stir evenly, pour into a mol...