a smfe x Alloy and its preparation method
A technology of alloys and alloying elements, which is applied in the preparation of SmFex alloys by reduction diffusion method and its preparation field, which can solve the problems of difficult to accurately control the samarium content of target alloys, restrict the development of samarium-iron-nitrogen permanent magnet materials, and the production process is long. Labor cost and auxiliary material consumption are reduced, washing time is shortened, and the effect of uniform distribution
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0032] (1) Selection of raw materials: The raw materials are samarium oxide (purity greater than 99.95%), samarium chloride (purity greater than 99%), iron powder (purity greater than 99.5%, size is 200 mesh) and metal calcium particles (purity greater than 99.5%) , particle size is 2 ~ 5mm).
[0033] (2) Raw material pretreatment: vacuum dehydrate calcium chloride at 400° C. for 1.5 h.
[0034] (3) After mixing samarium chloride, samarium oxide, iron powder and calcium particles evenly, charge the furnace.
[0035] (4) Vacuumize, after washing the furnace with high-purity argon for 3 times, fill it with high-purity argon to 0.98 atmospheres;
[0036] (5) After raising the temperature to 750° C. for 1.5 hours, then raising the temperature to 1100° C. for 3 hours, then turning off the power and cooling to room temperature.
[0037] (6) The product is crushed to 50 mesh, washed with water to separate the samarium-iron alloy and the reducing slag.
[0038] (7) The product is v...
Embodiment 2
[0051] A SmFe 9.0 The preparation method of the base alloy material is basically the same as in Example 1, except that the ratio of samarium oxide and samarium chloride is as follows (the ratio of samarium oxide: samarium chloride is 8):
[0052] The raw material formula of table 4 embodiment 2
[0053] Samarium oxide 29.8g Samarium chloride 3.7g
[0054] iron powder 88.3g Calcium particles 14.5g
[0055] 2. Process conditions are shown in Table 5:
[0056] The processing condition of table 5 embodiment 2
[0057] Samarium chloride treatment temperature 400℃ processing time 1.5h Mixing time 1.5h Charging furnace temperature 60℃ Heating rate 15℃ / min One-stage holding temperature 750℃ One-stage constant temperature time 1.5h Second stage holding temperature 1100℃ Two-stage constant temperature time 3h Broken particle size 50 mesh washing time 60min
[0058] 3. Results: The w...
Embodiment 3
[0062] A SmFe 6 The preparation method of the basic alloy material is basically the same as that of Example 1, the difference is only to adjust the amount of Fe powder added and the process conditions:
[0063] The raw material formula of table 7 embodiment 3
[0064] Samarium oxide 29.8g Samarium chloride 4.4g iron powder 56.7g Calcium particles 14.2g
[0065] 2. The process conditions are shown in Table 8:
[0066] The process condition of table 8 embodiment 3
[0067] Samarium chloride treatment temperature 400℃ processing time 1.5h Mixing time 1.5h Charging furnace temperature 60℃ Heating rate 15℃ / min One-stage holding temperature 750℃
[0068] One-stage constant temperature time 1.5h Second stage holding temperature 1050℃ Two-stage constant temperature time 4h Broken particle size 50 mesh washing time 60min
[0069] 3. Results: The weight of the product is 82g, the di...
PUM
Property | Measurement | Unit |
---|---|---|
particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com