A method for preparing a nanometer porous nickel-iron-sulfur alloy having a high catalytic oxygen evolution property through electrodeposition in a eutectic type ionic liquid

A nanoporous nickel and ionic liquid technology, applied in chemical instruments and methods, nanotechnology, nanotechnology, etc., can solve the problems that limit the wide application of nickel-iron-sulfur alloys, difficulty in performance control, and high technical requirements for equipment, and achieve product quality Stable, inexpensive, evenly distributed effect

Active Publication Date: 2017-11-10
KUNMING UNIV OF SCI & TECH
View PDF5 Cites 16 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0003] The traditional methods for preparing nickel-iron-sulfur alloys mainly include solvothermal method, hydrothermal method, liquid phase method, electrodeposition method, mechanical method, etc. These methods often have high temperature, high consumption, and difficulty in control during the preparation process. Disadvantages, great damage to the environment, high technical requirements for equipment, difficult performance control and many other problems limit the wide application of nickel-iron-sulfur alloys

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • A method for preparing a nanometer porous nickel-iron-sulfur alloy having a high catalytic oxygen evolution property through electrodeposition in a eutectic type ionic liquid
  • A method for preparing a nanometer porous nickel-iron-sulfur alloy having a high catalytic oxygen evolution property through electrodeposition in a eutectic type ionic liquid
  • A method for preparing a nanometer porous nickel-iron-sulfur alloy having a high catalytic oxygen evolution property through electrodeposition in a eutectic type ionic liquid

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0023] The method for preparing nanoporous nickel-iron-sulfur alloy with high catalytic oxygen evolution performance by electrodeposition in the eutectic ionic liquid, the specific steps are as follows:

[0024] (1) Electrolyte configuration: Mix quaternary ammonium salt (choline chloride) and alcohols (ethylene glycol) in a molar ratio of 1:2 to obtain a eutectic ionic liquid, and then mix the nickel salt precursor (6 Hydrate nickel chloride), iron salt precursor (ferric chloride hexahydrate) and sulfur salt precursor (thiourea) are added to the eutectic ionic liquid, and the ionic liquid iron salt-nickel salt is obtained after thorough stirring and mixing -Sulfur salt composite electrolyte, wherein the molar ratio of nickel salt precursor, iron salt precursor, and sulfur salt precursor is 0.1:0.03:0.02, and the solid-liquid ratio of nickel salt precursor and eutectic ionic liquid is 0.1: 50mol / mL;

[0025] (2) Surface treatment of the working electrode: The nickel matrix (1...

Embodiment 2

[0029] The method for preparing nanoporous nickel-iron-sulfur alloy with high catalytic oxygen evolution performance by electrodeposition in the eutectic ionic liquid, the specific steps are as follows:

[0030] (1) Electrolyte configuration: Mix quaternary ammonium salt (choline chloride) and amide (urea) at a molar ratio of 1:3 to obtain a eutectic ionic liquid, and then mix the nickel salt precursor (hexahydrate chloride Nickel), iron salt precursor (ferric chloride hexahydrate) and sulfur salt precursor (thiourea) are added to the eutectic ionic liquid, and the ionic liquid iron salt-nickel salt-sulfur salt is obtained after thorough stirring and mixing Composite electrolyte, wherein the molar ratio of nickel salt precursor, iron salt precursor and sulfur salt precursor is 0.1:0.03:0.02, and the solid-liquid ratio of nickel salt precursor and eutectic ionic liquid is 0.1:50mol / mL ;

[0031] (2) Surface treatment of working electrode: nickel foam (1.5cm×1.5cm×0.1cm) was us...

Embodiment 3

[0035] The method for preparing nanoporous nickel-iron-sulfur alloy with high catalytic oxygen evolution performance by electrodeposition in eutectic ionic liquid, the specific steps are as follows:

[0036] (1) Electrolyte configuration: Mix quaternary ammonium salt (choline chloride) and amide (acetamide) at a molar ratio of 1:4 to obtain a deep eutectic ionic liquid, and then nickel salt precursor (chlorine hexahydrate Nickel chloride), iron salt precursor (ferric chloride hexahydrate) and sulfur salt precursor (thiourea) were added to the eutectic ionic liquid, and after thorough stirring and mixing, the ionic liquid iron salt-nickel salt-sulfur Salt composite electrolyte, wherein the molar ratio of nickel salt precursor, iron salt precursor, and sulfur salt precursor is 0.1:0.05:0.02, and the solid-liquid ratio of nickel salt precursor to eutectic ionic liquid is 0.1:50mol / mL;

[0037] (2) Surface treatment of working electrode: use copper sheet (1.5cm×1.5cm×0.1cm) as w...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention relates to a method for preparing a nanometer porous nickel-iron-sulfur alloy having a high catalytic oxygen evolution property through electrodeposition in a eutectic type ionic liquid, and belongs to the technical field of material preparation. The method includes fully mixing a quaternary ammonium salt with an alcohol or an amide to obtain the eutectic type ionic liquid, then adding a nickel salt precursor, an iron salt precursor and a sulfur salt precursor into the eutectic type ionic liquid, fully stirring and mixing the mixture to obtain an ionic liquid iron salt-nickel salt-sulfur salt composite electrolyte, subjecting a copper or nickel substrate that is adopted as a working electrode to repeated soaking with dilute hydrochloric acid and absolute ethanol, washing the working electrode with deionized water, then drying the working electrode, keeping the working electrode for later use, performing constant-potential electrodeposition by adopting a three-electrode system, washing the working electrode substrate after the electrodeposition with absolute ethanol and distilled water, and drying the working electrode substrate, and then a nanometer porous nickel-iron-sulfur alloy material film can be obtained on the surface of the working electrode substrate. A nickel-iron-sulfur alloy nanometer porous material having a high catalytic oxygen evolution property can be prepared by electrodeposition through the method.

Description

technical field [0001] The invention relates to a method for preparing nano-porous nickel-iron-sulfur alloy with high catalytic oxygen evolution performance by electrodeposition in eutectic ionic liquid, and belongs to the technical field of material preparation. Background technique [0002] Nickel and its alloy catalytic materials have become the research hotspot of oxygen evolution electrode materials due to their low cost, wide source, high catalytic oxygen evolution activity and strong corrosion resistance. They are recognized as ideal electrode materials that are expected to replace precious metals. In nickel-based alloys, the catalytic performance of nickel-iron alloys is superior to other nickel-based catalysts due to the formation of catalytically active nickel hydroxide in the catalytic process. Due to the poor electrical conductivity between metals, the catalytic performance of NiFe-based catalytic materials cannot be further improved. In order to solve this prob...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): B01J27/049B01J35/10B01J37/34B82Y30/00C25D3/66
CPCB01J27/049B01J35/065B01J35/10B01J37/348B82Y30/00C25D3/665
Inventor 张启波高明远杨闯华一新徐存英李坚李艳
Owner KUNMING UNIV OF SCI & TECH
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products