Preparation method of sodium sulfide

A technology of sodium sulfide and raw coal, applied in alkali metal sulfide/polysulfide, chemical industry, sustainable manufacturing/processing, etc., can solve the problem of incomplete reaction of mirabilite, pulverized coal, incomplete calcination of pulverized coal, and output of sodium sulfide Low and other problems, to achieve the effect of improving the conversion rate of raw materials, reducing the content of SO2, and reducing the content of SO2

Inactive Publication Date: 2018-11-30
铜陵铜冠环保科技有限公司
View PDF0 Cites 2 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

The existing mixture of Glauber's salt and coal powder is only simple mixing, and Glauber's salt is usually irregular flakes or granules. Simple mixing has a small contact area. Powder calcination is not complete, a large amount of waste gas is produced, and the output of sodium sulfide is low
The above two kinds of industrial sodium sulfide produced have the problems of many impurities and high iron content, which will affect the quality of the final product during the application process.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0015] A method for preparing sodium sulfide, comprising the steps of:

[0016] a. Put the raw coal into the ball mill and grind it into powder, then add the raw coal powder and sodium sulfate into the mixer, mix and stir evenly, and get the mixture for later use, wherein the raw coal powder and sodium sulfate are added in a ratio of 1:2 ;

[0017] b. Spray the mixed material that has been stirred into the calciner, maintain the slight negative pressure atmosphere in the calciner, so that the calcining temperature is maintained at 1000 ° C, and the calcining time is 30 minutes to obtain a sodium sulfide alkali billet for use;

[0018] c. The sodium sulfide alkali billet is melted into a liquid by heat, and the alkali billet is washed with water into a solution with a sodium sulfide content greater than 300g / L, and left to stand for purification and clarification for 20 hours to obtain a reduction leaching solution;

[0019] d. Evaporate the leaching solution to about 250g / L t...

Embodiment 2

[0023] A method for preparing sodium sulfide, comprising the steps of:

[0024] a. Put the raw coal into the ball mill and grind it into a powder, then add the raw coal powder and sodium bicarbonate into the mixer, mix and stir evenly, and get the mixture for later use, wherein the raw coal powder and sodium bicarbonate are added in a ratio of 1:2.5 ;

[0025] b. Spray the mixed material that has been stirred into the calciner, maintain the slight negative pressure atmosphere in the calciner, so that the calcining temperature is maintained at 1020°C, and the calcining time is 35min, so as to obtain a sodium sulfide alkali billet for use;

[0026] c. The sodium sulfide alkali billet is melted into a liquid by heat, and the alkali billet is washed with water into a solution with a sodium sulfide content greater than 300g / L, and left to stand for purification and clarification for 25 hours to obtain a reduction leaching solution;

[0027] d. Evaporate the leaching solution to ab...

Embodiment 3

[0031] A method for preparing sodium sulfide, comprising the steps of:

[0032] a. Put the raw coal into the ball mill and grind it into a powder, then add the raw coal powder and sodium bicarbonate powder into the mixer, mix and stir evenly, and get the mixture for later use, wherein the raw coal powder and sodium bicarbonate powder are added in a ratio of 1:3 ;

[0033] b. Spray the mixed material that has been stirred into the calciner, maintain the slight negative pressure atmosphere in the calciner, so that the calcining temperature is maintained at 1050° C., and the calcining time is 40 minutes to obtain a sodium sulfide alkali billet for use;

[0034] c. The sodium sulfide alkali billet is melted into a liquid by heat, and the alkali billet is washed with water into a solution with a sodium sulfide content greater than 300g / L, and left to stand for purification and clarification for 30 hours to obtain a reduction leaching solution;

[0035] d. Evaporate the leaching so...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention discloses a preparation method of sodium sulfide, the preparation method comprises the following steps: a, adding raw coal powder and anhydrous sodium sulphate into a mixer to obtain a mixture for standby use; b, spraying the mixture into a calcining furnace to obtain sodium sulfide alkali billet for standby use; c, thermally melting the sodium sulfide alkali billet into a liquid toobtain a reducing leaching solution; d, evaporating the reducing leaching solution to about 250 g / L to obtain a sodium sulfide semi-finished product leaching solution; e, removing heavy metal ions inthe leaching solution until the total content of metal ions in the leaching solution is less than that of 10ppm filtrate; f, pumping the filtrate into a crystallization tank, and performing rapid vacuum freeze-crystallizing and centrifugal dehydration to obtain high-purity sodium sulfide. The raw coal powder is ground and crushed, so that the contact area of the raw coal powder and the anhydrous sodium sulphate is bigger, the reaction is more sufficient when heating and reducing, and the yield of the sodium sulfide is improved; by negative pressure calcination and temperature control, the content of soluble impurities of the product can be reduced, the conversion rate of raw materials can be improved, consumption is reduced, and the effect of energy saving and consumption reduction can beobtained.

Description

technical field [0001] The invention relates to the technical field of sodium sulfide preparation, in particular to a preparation method of sodium sulfide. Background technique [0002] Sodium sulfide is also called smelly alkali, smelly soda, yellow alkali, and alkali sulfide. Sodium sulfide is an inorganic compound, and pure sodium sulfide is a colorless crystalline powder; it has strong moisture absorption and is easily soluble in water; the aqueous solution is strongly alkaline; it will cause burns when it touches the skin and hair; therefore, sodium sulfide is commonly known as alkali sulfide. At present, there are two main production methods of industrial sodium sulfide in my country, one is the main production method - Glauber's salt calcination method; the other is the secondary production method - precipitation of barium sulfate and secondary production of sodium sulfide. The existing mixture of Glauber's salt and coal powder is only simple mixing, and Glauber's sa...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): C01B17/26
CPCC01B17/26Y02P20/10
Inventor 许玮唐雁戴正亮朱世银宋晓轩
Owner 铜陵铜冠环保科技有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products