Flotation method of brass ore-containing complex lead-zinc sulphide ore
A chalcopyrite type, sulfide ore technology, applied in flotation, solid separation, etc., to achieve the effect of no pollution to the environment, high recovery rate, and beneficial to recycling
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0030] A chalcopyrite-bearing complex lead-zinc sulfide ore in Yunnan. The main metal minerals of this ore are chalcopyrite, galena, sphalerite and pyrite. The main gangue minerals are quartz, calcite and so on. The results of the multi-element analysis of the raw ore are shown in Table 1.
[0031] Table 1 Multi-element analysis of raw ore
[0032]
[0033] use as figure 1 Shown technological process, concrete technological parameter is as follows:
[0034] ① Grinding process: add lime to keep the pH value at 10, add 300g / t raw ore of sodium pyrosulfite, and adjust the pulp potential to 220mV relative to the hydrogen standard potential. Add 500g / t raw ore of zinc sulfate, 10g / t raw ore of ethyl xanthate formate, and 10g / t raw ore of ethyl disulfide. Grinding is carried out with a wet ball mill, and the particle size of the grinding product is -0.074mm, accounting for 65%.
[0035] ②Mixed flotation of copper-lead minerals: keep the pH of the pulp at pH=10, add 10g / t raw...
Embodiment 2
[0045] A chalcopyrite-bearing complex lead-zinc sulfide ore in Hunan, the main metal minerals of this ore are chalcopyrite, galena, sphalerite and pyrite. The main gangue minerals are quartz, calcite and so on. The results of the multi-element analysis of the raw ore are shown in Table 2.
[0046] Table 2 Multi-element analysis of raw ore
[0047]
[0048] use as figure 1 Shown technological process, concrete technological parameter is as follows:
[0049] ① Grinding process: Add lime to keep the pH value at 11, add 500g / t raw ore of sodium pyrosulfite, and adjust the pulp potential to 260mV relative to the hydrogen standard potential. Add 700g / t raw ore of zinc sulfate, 20g / t raw ore of ethyl xanthate formate, and 20g / t raw ore of ethyl disulfide. Grinding is carried out with a wet ball mill, and the particle size of the grinding product is -0.074mm, accounting for 70%.
[0050] ②Mixed flotation of copper-lead minerals: keep the pH of the pulp at pH=11, add 10g / t raw ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology