Wood surface corrosion control method

A wood surface and wood technology, applied in the field of chemical science, can solve the problems of unfavorable environmental protection and the toxicity of preservatives, and achieve the effects of short anti-corrosion treatment time, good anti-corrosion effect and strong penetration

Inactive Publication Date: 2015-06-24
HAIMEN JINQILIN REDWOOD INVESTMENT DEV
View PDF0 Cites 6 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

At present, the wood preservatives used in countries all over the world are mainly CCA preservatives. This kind of preservatives are toxic because they contain arsenic, chromium and other substances, which is not conducive to environmental protection. In some countries, their use has been strictly restricted.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0026] A kind of anticorrosion method of wood surface, this method is:

[0027] (1) Dry the wood until the moisture content is about 18%;

[0028] (2) Inject the following preservatives into the wood under vacuum and high pressure: 3.5 parts of propylene glycol, 40 parts of propylene carbonate, 2 parts of DCOIT, 20 parts of p-chloro-m-xylenol, alkyl dimethyl benzyl chloride 3 parts of ammonium chloride, 2 parts of sodium chloride, 2 parts of sodium chlorate, 2 parts of potassium bromide, 7.5 parts of bronopol, 40 parts of dithiocyanomethane, 110 parts of fatty alcohol polyvinyl chloride ether;

[0029] (3) After adding the preservative, the wood was subjected to high-temperature qualitative treatment for 8 hours;

[0030] (4) After the high-temperature qualitatively treated wood is air-dried, the anti-corrosion treated wood can be obtained.

Embodiment 2

[0032] A kind of anticorrosion method of wood surface, this method is:

[0033] (1) Dry the wood until the moisture content is about 18%;

[0034] (2) Inject the following preservatives into the wood under vacuum and high pressure: 3.8 parts of propylene glycol, 44 parts of propylene carbonate, 2.5 parts of DCOIT, 25 parts of p-chloro-m-xylenol, alkyl dimethyl benzyl chloride 2 parts of ammonium chloride, 2.2 parts of sodium chloride, 2.3 parts of sodium chlorate, 2.2 parts of potassium bromide, 7.9 parts of bronopol, 43 parts of dithiocyanomethane, 116 parts of fatty alcohol polyvinyl chloride ether;

[0035] (3) After adding the preservative, the wood was subjected to high-temperature qualitative treatment for 10 hours;

[0036] (4) After the high-temperature qualitatively treated wood is air-dried, the anti-corrosion treated wood can be obtained.

Embodiment 3

[0038] A kind of anticorrosion method of wood surface, this method is:

[0039] (1) Dry the wood until the moisture content is about 18%;

[0040] (2) Inject the following preservatives into the wood under vacuum and high pressure: 2 parts of propylene glycol, 30 parts of propylene carbonate, 1 part of DCOIT, 10 parts of p-chloro-m-xylenol, alkyl dimethyl benzyl chloride 1 part of ammonium, 1 part of sodium chloride, 1 part of sodium chlorate, 1 part of potassium bromide, 5 parts of bronopol, 35 parts of dithiocyanomethane, 108 parts of fatty alcohol polyvinyl chloride ether;

[0041] (3) After adding the preservative, the wood is subjected to high-temperature qualitative treatment for 12 hours;

[0042] (4) After the high-temperature qualitatively treated wood is air-dried, the anti-corrosion treated wood can be obtained.

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention discloses a wood surface corrosion control method. The method comprises the following steps: (1) drying the wood until the water content is about 18%; (2) injecting the preservatives, namely 2-4 parts of propylene glycol, 30-48 parts of propene carbonate, 1-2.3 part of DCOIT, 10-25 parts of p-chloroxylenol, 1-4 parts of alkyl dimethyl benzyl ammonium chloride, 1-2.8 part of sodium chloride, 1-3 parts of sodium chlorate, 1-3 parts of potassium bromide, 5-8 parts of bronopol, 35-46 parts of dithiocyano-methane and 108-116 parts of fatty alcohol polyvinyl chloride ether in part by weight, into the wood under the vacuum high pressure condition; (3) performing high-temperature qualitative treatment for 6-12 hours on the wood after the preservatives are added; and (4) carrying out air drying on the high-temperature qualitatively treated wood to obtain the wood subjected to preservative treatment. The corrosion control method disclosed by the invention is good in corrosion control effect, the preservatives can permeate into the part being 1-2mm of the wood surface, and good mold prevention and corrosion resistance are obtained; the wood is strong in waterproof durability, is loss resistant and long in residual action, the raw materials is easily available, and the cost can be saved.

Description

technical field [0001] The invention relates to an anticorrosion method, in particular to an anticorrosion method for wood surfaces, and belongs to the field of chemical science. Background technique [0002] Wood is an organic material with obvious biological characteristics, and is easily attacked by organisms such as bacteria, insects, and marine borers. Therefore, the long-term use of wood, especially long-term outdoor use, is greatly restricted. Decay organisms cause rot in wood, causing it to become damaged. Before use, according to different application environments, choose suitable preservatives and carry out proper treatment, which can effectively delay wood decay. Carrying out anti-corrosion treatment on wood and prolonging the service life of wood is one of the important ways to save wood and protect forest resources. At present, the wood preservatives used in countries all over the world are mainly CCA preservatives, which are toxic due to arsenic, chromium an...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): B27K3/08B27K3/52A01N59/08A01P1/00A01P3/00A01N33/12
CPCB27K3/08A01N33/12A01N59/08B27K3/0214B27K3/52B27K5/001B27K2240/00B27K2240/20B27K2240/70
Inventor 孙建豪
Owner HAIMEN JINQILIN REDWOOD INVESTMENT DEV
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products