A kind of pia waste material modified alkyd resin and preparation method thereof
An alkyd resin and waste technology, applied in the direction of coating, can solve the problems of poor weather resistance, corrosion resistance and water resistance, and the hardness of the coating film is not ideal, achieve good compatibility and avoid gel phenomenon , the effect of improving hydrolysis resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] A kind of PIA waste material modified alkyd resin proposed by the present invention, its raw material comprises the following components by weight: 10 parts of acrylic acid, 15 parts of methacrylic acid, 20 parts of methyl methacrylate, 10 parts of styrene, 35 parts of castor oil 25 parts of trimethylolpropane, 2 parts of 2,2,4-trimethyl-1,3-pentanediol, 25 parts of 1,4-cyclohexanedicarboxylic acid, 6 parts of PIA waste, 10 parts of trimellitic anhydride , 1 part of triethylamine, 10 parts of ethylene glycol monobutyl ether, 10 parts of propylene glycol monobutyl ether, 8 parts of lauric acid, 0.01 part of catalytic promoter, 2 parts of benzoyl peroxide, and 20 parts of water.
[0031] The preparation method of described PIA waste material modified alkyd resin that the present invention proposes may further comprise the steps:
[0032] S1. Under the protection of nitrogen, mix castor oil, trimethylolpropane, and 2,2,4-trimethyl-1,3-pentanediol evenly, heat up to 148°C u...
Embodiment 2
[0037] A kind of PIA waste material modified alkyd resin that the present invention proposes, its raw material comprises the following components by weight: 20 parts of acrylic acid, 7 parts of methacrylic acid, 45 parts of methyl methacrylate, 3 parts of styrene, 40 parts of castor oil 20 parts of trimethylolpropane, 5 parts of 2,2,4-trimethyl-1,3-pentanediol, 15 parts of 1,4-cyclohexanedicarboxylic acid, 8 parts of PIA waste, 6 parts of trimellitic anhydride , 5 parts of triethylamine, 3 parts of ethylene glycol monobutyl ether, 35 parts of propylene glycol monobutyl ether, 2 parts of lauric acid, 0.05 parts of catalytic promoter, 1 part of benzoyl peroxide, and 50 parts of water.
[0038] The preparation method of described PIA waste material modified alkyd resin that the present invention proposes may further comprise the steps:
[0039] S1. Under the protection of nitrogen, mix castor oil, trimethylolpropane, and 2,2,4-trimethyl-1,3-pentanediol evenly, raise the temperatu...
Embodiment 3
[0044] A kind of PIA waste material modified alkyd resin proposed by the present invention, its raw material comprises the following components by weight: 14 parts of acrylic acid, 11 parts of methacrylic acid, 28 parts of methyl methacrylate, 8.5 parts of styrene, 38 parts of castor oil 24.3 parts of trimethylolpropane, 3.7 parts of 2,2,4-trimethyl-1,3-pentanediol, 21 parts of 1,4-cyclohexanedicarboxylic acid, 7.2 parts of PIA waste, 8.7 parts of trimellitic anhydride , 2.9 parts of triethylamine, 8.2 parts of ethylene glycol monobutyl ether, 18 parts of propylene glycol monobutyl ether, 5 parts of lauric acid, 0.036 parts of catalytic aid, 1.7 parts of benzoyl peroxide, and 32 parts of water.
[0045] The preparation method of described PIA waste material modified alkyd resin that the present invention proposes may further comprise the steps:
[0046] S1. Under the protection of nitrogen, mix castor oil, trimethylolpropane, and 2,2,4-trimethyl-1,3-pentanediol evenly, heat up...
PUM
| Property | Measurement | Unit |
|---|---|---|
| hardness | aaaaa | aaaaa |
| tack-free time | aaaaa | aaaaa |
| adhesivity | aaaaa | aaaaa |